Lithium ion supply electrode for real-time microscopic analysis and method for manufacturing same
By using a solid electrolyte layer and a lithium layer with a metal protective layer in the lithium ion supply electrode, the problem of lithium oxidation and equipment environmental adaptability is solved, and real-time analysis effects of high lithium ion conductivity and clear images are achieved.
Patent Information
- Application Number
- CN202280092472.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-07
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-08
AI Technical Summary
Existing lithium ion supply electrodes are easily oxidized in the air, resulting in a reduction in lithium ion conductivity, making it impossible to conduct real-time analysis on light and vibration sensitive equipment such as transmission electron microscopes, and liquid electrolytes are difficult to exist in high vacuum environments, resulting in image Not clear.
Using a lithium ion supply electrode with a solid electrolyte layer and a lithium layer with a metal protective layer, a laminated material is prepared by forming a liquid phase lithium layer under inert gas conditions and adding a metal protective layer, and is etched using a focused ion beam device. Specific shape to prevent lithium oxidation and adapt to the device environment.
It realizes the use of solid electrolytes with high lithium ion conductivity in charging and discharging environments to prevent lithium oxidation. It is suitable for the analysis of light- and vibration-sensitive devices and provides clear microstructure images.
Smart Images

Figure CN118749064A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a lithium ion supply electrode for real-time transmission electron microscopy and a method for manufacturing the same. The present disclosure relates to a lithium ion supply electrode and a method for manufacturing the same, the electrode comprising a metal-containing protective layer to inhibit oxidation of lithium when a lithium secondary battery material is loaded into a holder for real-time analysis. Background Art
[0002] At present, most lithium ion supply electrodes for transmission electron microscope (TEM) analysis are made by wetting metal tips with liquid lithium in a glove box. The metal tip is loaded into the TEM holder in the air for a short time. For this short time, lithium is exposed to the air and oxidized to lithium oxide (Li2O). This lithium oxide used as a solid electrolyte is contacted with the lithium secondary battery material, and a voltage is applied for analysis. Compared with the materials currently being studied and used as solid electrolytes, lithium oxide (Li2O) has a significantly lower lithium ion conductivity. Compared with the actual battery environment, this lithium ion conductivity difference will produce overvoltage. Since the conditions of the test electrode are different from those of the actual electrode, this test cannot be regarded as a test of the actual lithium secondary battery material using a solid electrolyte. In addition, in the case of making a lithium ion supply electrode by wetting a metal tip with liquid lithium in a glove box, the glove box must be located near the microscope so that the electrode can be loaded into the holder in a short time to prevent oxidation of lithium in the air. However, since the transmission electron microscope is particularly sensitive to light and vibration, the microscope and the glove box are not easy to be installed close to each other due to the vibration generated by the pump of the glove box.
[0003] In addition, a liquid holder for providing a liquid environment is required to perform real-time charge and discharge tests in a liquid environment. However, due to the high price of the equipment, it is difficult to use a liquid holder. In addition, since the TEM images using a liquid holder are obtained from an electron beam transmitted through a liquid environment, these images may be relatively unclear and blurred compared to images obtained from an electron beam passing through a vacuum environment. However, without using a liquid holder, it is difficult to perform real-time microscopic analysis with a liquid electrolyte on a metal tip to obtain a clean image, because the liquid electrolyte cannot exist in the high vacuum environment of a transmission electron microscope, and the liquid electrolyte is likely to be solidified by the electron beam.
[0004] Therefore, in order to perform real-time analysis of lithium secondary battery materials, it is necessary to develop a lithium ion supply electrode that can be maintained in air for a long time and uses a solid electrolyte with high lithium ion conductivity. Summary of the invention Technical issues
[0005] The present disclosure is made in view of the problems arising in the related art, and the purpose of the present disclosure is to provide a lithium ion supply electrode and a method for manufacturing the same. Through the electrode and method disclosed in the present disclosure, a solid electrolyte with high lithium ion conductivity is used for real-time analysis of secondary battery materials in a charging and discharging environment, and lithium is not oxidized but remains unchanged during the process of loading the electrode into a holder.
[0006] In addition, a small lithium ion supply electrode is provided, which can be used to analyze microstructural changes and interface reactions of lithium secondary batteries by using an apparatus sensitive to light and vibration, such as a transmission electron microscope (TEM). Technical Solution
[0007] According to one aspect of the present disclosure, a lithium ion supply electrode is provided, comprising: a solid electrolyte layer, the solid electrolyte layer containing a solid electrolyte; a lithium layer, the lithium layer formed on the solid electrolyte layer and containing lithium; and a protective layer, the protective layer formed on the lithium layer and containing a metal.
[0008] In addition, the lithium layer may have a thickness of 0.5 μm to 10 μm.
[0009] The metal included in the protective layer may be one or more metals selected from the group consisting of copper (Cu), gold (Au), silver (Ag), and nickel (Ni).
[0010] In addition, the metal included in the protective layer may be copper (Cu).
[0011] In addition, the protective layer may have a thickness of 0.5 μm to 10 μm.
[0012] In addition, the area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases.
[0013] Furthermore, the solid electrolyte layer may have any one shape selected from the group consisting of a circular cone shape, an elliptical cone shape, a flat plate shape, and a polygonal pyramid shape.
[0014] In addition, the solid electrolyte may be one or more electrolytes selected from the group consisting of an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a phosphide-based solid electrolyte, a silicide-based solid electrolyte, and a combination thereof.
[0015] Furthermore, the solid electrolyte layer may have a thickness of 0.5 μm to 85 mm.
[0016] In addition, the lithium ion supply electrode can be used to analyze the lithium secondary battery material during the charging and discharging process of the lithium secondary battery using any one selected from the group consisting of a transmission electron microscope (TEM), a scanning electron microscope (SEM), an optical microscope (OM) and a scanning probe microscope (SPM).
[0017] According to another aspect of the present disclosure, a method for manufacturing a lithium ion supply electrode is provided, the method comprising: (a) forming a liquid lithium layer on a solid electrolyte layer under inactive gas conditions and at a temperature at or above the melting point of lithium, and forming a protective layer containing a metal on the liquid lithium layer, thereby preparing a laminated material including a solid electrolyte layer, a lithium layer and a protective layer; and (b) separating a portion of the laminated material using a focused ion beam device at a temperature below the melting point of lithium so that the separated portion has a predetermined shape, thereby producing a lithium ion supply electrode including a solid electrolyte layer, a lithium layer and a protective layer.
[0018] Furthermore, step (a) may be performed at a temperature ranging from 180.5°C to 500°C.
[0019] In the method, the steps may include: (a-1) wetting a solid electrolyte layer with liquid lithium to form a laminate of a solid electrolyte layer and a liquid lithium layer; and (a-2) placing a protective layer containing a metal on the liquid lithium layer to prepare a laminate of a solid electrolyte layer, a lithium layer and a protective layer.
[0020] Step (a) may further include step (a-1') performed between step (a-1) and step (a-2): (a-1') adjusting the thickness of the liquid lithium layer by adding liquid lithium to the liquid lithium layer or removing some liquid lithium from the liquid lithium layer at a temperature at or above the melting point of lithium.
[0021] In the method, step (b) may include: (b-1) using a focused ion beam device, etching a laminate material consisting of a solid electrolyte layer, a lithium layer and a protective layer into a bridge-shaped pattern when viewed from above the protective layer; (b-2) etching off one of the left and right ends of the bridge-shaped pattern and etching off the lower portion of the bridge-shaped pattern; (b-3) bonding a probe to the surface of the protective layer of the bridge-shaped pattern, etching the left or right end and the lower portion from the bridge-shaped pattern; and (b-4) etching off the remaining unetched ends of the left and right ends of the bridge-shaped pattern, thereby obtaining a lithium ion supply electrode comprising a protective layer, a lithium layer and a solid electrolyte layer and bonded to the probe.
[0022] The method may further include steps (c) and (d) performed after step (b-4): (c) bonding a protective layer and a lithium layer of a lithium ion supply electrode to the metal tip, but not bonding a portion or all of the solid electrolyte layer to the metal tip; and (d) etching the solid electrolyte layer so that a cross-sectional area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases.
[0023] The method may further include a step (c') performed before step (c): (c') bringing the lithium ion supply electrode bonded to the probe close to the metal tip, and rotating the probe so that the surface of the protective layer of the laminate material bonded to the probe, the surface of the lithium layer, and the surface of the solid electrolyte layer face the metal tip.
[0024] In another aspect of the present disclosure, a method for real-time analysis of lithium secondary battery materials is provided, the method comprising: (1) loading a lithium ion supply electrode into a first retainer of a real-time bias retainer; (2) loading a material for a lithium secondary battery into a second retainer; and (3) bringing a solid electrolyte of the lithium ion supply electrode into contact with the material, and applying a voltage or current to the lithium ion supply electrode and the material to analyze the changes in the structure and interface of the material in real time using a microscope during charging or discharging.
[0025] In addition, the material for the lithium secondary battery may be any one selected from the group consisting of a negative electrode material, an electrolyte, a positive electrode material, and a current collector.
[0026] Furthermore, the microscope may be any one selected from the group consisting of a transmission electron microscope (TEM), a scanning electron microscope (SEM), an optical microscope (OM), and a scanning probe microscope (SPM). Beneficial Effects
[0027] The lithium ion supply electrode disclosed herein is used for real-time analysis of lithium secondary battery materials in a charging and discharging environment. To this end, the lithium ion supply electrode uses a solid electrolyte with high lithium ion conductivity. In addition, the lithium ion supply electrode disclosed herein has the effect of maintaining the amount of lithium by preventing lithium oxidation when the electrode is loaded into a holder.
[0028] In addition, since the lithium ion supply electrode of the present invention has the advantage of preventing lithium oxidation in a short time, a glove box is not required. Therefore, the lithium ion supply electrode of the present invention can be used to analyze the structural changes and interface responses of lithium secondary battery materials using equipment sensitive to light and vibration (e.g., transmission electron microscope). BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Since the accompanying drawings are mentioned in describing exemplary embodiments of the present disclosure, the technical spirit of the present disclosure should not be construed as being limited to the accompanying drawings, wherein:
[0030] Figure 1 is a schematic diagram showing a laminated material with a protective layer and a laminated material without a protective layer according to one embodiment of the present disclosure.
[0031] 2 is a schematic diagram showing a lithium ion supply electrode before and after a probe is rotated 180° in a focused ion beam apparatus when the lithium ion supply electrode is manufactured by a manufacturing method according to one embodiment of the present disclosure.
[0032] 3 is images taken using a scanning electron microscope (SEM) in a focused ion beam apparatus, and these images show the degree of oxidation of lithium in each laminated material prepared according to Example 1 and Comparative Example 1. FIG.
[0033] 4 are images taken using a scanning electron microscope (SEM) in a focused ion beam apparatus, and the images show a process of manufacturing a lithium ion supplying electrode according to Example 1 using the focused ion beam apparatus.
[0034] 5 is a diagram illustrating a process of loading a prepared lithium ion supplying electrode and a working electrode (current collector material) in a real-time bias holder for plating reaction analysis of a lithium secondary battery current collector according to Example 2. Referring to FIG.
[0035] FIG. 6 is a graph showing the experimental results of Example 2 when lithium-phobic Cu is used as a working electrode.
[0036] FIG. 7 is a graph showing the experimental results of Example 2 when lithium-phobic Ni is used as a working electrode.
[0037] FIG. 8 is a graph showing the experimental results of Example 2 when lithiophobic Ni coated with lithiophilic Ag is used as a working electrode.
[0038] 9 is a view showing lithium particles generated during the precipitation reaction analysis of Example 2 when lithium-phobic Cu is used as a working electrode, and showing a change in shape of a lithium ion supplying electrode when the electrode is exposed to air after the analysis. DETAILED DESCRIPTION
[0039] Hereinafter, embodiments of the present invention are described in detail with reference to the accompanying drawings in such a manner that a person having ordinary skill in the art can easily implement the present invention.
[0040] The description given below is not intended to limit the present invention to a specific embodiment. With respect to describing the present invention, when it is determined that the detailed description of the related known technology unnecessarily obscures the gist of the present invention, the detailed description may be omitted.
[0041] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the scope of the present invention. As used herein, unless the context clearly indicates otherwise, the singular forms "a" and "an" and "the" also include plural forms. It will be further understood that the terms "comprise" or "have" used in this specification specify the presence of stated features, integers, steps, operations, elements and / or combinations thereof, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements and / or combinations thereof.
[0042] The terms "first", "second", etc. including ordinal numbers used in the specification may be used to distinguish one component from another component, but unless otherwise specified, the order or priority of the components is not limited by these terms. These terms are only used for the purpose of distinguishing one component from another component. For example, without departing from the scope of the present invention, the first component may be referred to as the second component, and the second component may also be referred to as the first component.
[0043] Furthermore, when it is mentioned that one component is "formed" or "stacked" on another component, it should be understood that one component may be directly attached or stacked on a front surface or one surface of another component, or an additional component may be disposed therebetween.
[0044] Hereinafter, a lithium ion supply electrode for real-time microscopic analysis and a method for manufacturing the same will be described in detail. However, these are described only as embodiments, and the present invention is not limited thereto but only by the scope of the appended claims.
[0045] Figure 1 is a schematic diagram showing a laminated material with a protective layer and a laminated material without a protective layer according to one embodiment of the present disclosure.
[0046] See also Figure 1 The present disclosure provides a lithium ion supply electrode, which includes: a solid electrolyte layer, which contains a solid electrolyte; a lithium layer, which is formed on the solid electrolyte layer and contains lithium; and a protective layer, which is formed on the lithium layer and contains a metal.
[0047] In addition, the thickness of the lithium layer may be in the range of 0.5 μm to 10 μm, preferably in the range of 1 μm to 8 μm, and more preferably in the range of 2 μm to 6 μm. When the thickness is less than 0.5 μm, not only is the lithium ion supply insufficient, but also a smooth interface is not formed between the solid electrolyte layer and the lithium layer and between the lithium layer and the protective layer. In addition, air may penetrate into the empty space and cause oxidation of lithium. When the thickness is greater than 10 μm, etching is time-consuming because the lithium ion supply electrode is manufactured using a focused ion beam device. In addition, the greater the etching amount, the more excessive the focused ion beam device is used.
[0048] The metal included in the protective layer may be one or more metals selected from the group consisting of copper (Cu), gold (Au), silver (Ag), and nickel (Ni).
[0049] In addition, the metal included in the protective layer may be copper (Cu).
[0050] In addition, the thickness of the protective layer may be in the range of 0.5 μm to 10 μm, preferably in the range of 4 μm to 8 μm, and more preferably in the range of 5 μm to 7 μm. When the thickness is less than 0.5 μm, it is difficult to handle with tweezers in a glove box, and it is insufficient to protect lithium metal from damage caused by the Ga ion beam in a focused ion beam device. When the thickness is greater than 10 μm, etching is time-consuming when a lithium ion supply electrode is manufactured using a focused ion beam device. In addition, the greater the etching amount, the more overused the focused ion beam device is.
[0051] In addition, the cross-sectional area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases.
[0052] Furthermore, the solid electrolyte layer may have any one shape selected from the group consisting of a circular cone shape, an elliptical cone shape, a flat plate shape, and a polygonal pyramid shape.
[0053] In addition, the solid electrolyte may be one or more electrolytes selected from the group consisting of an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a phosphide-based solid electrolyte, a silicide-based solid electrolyte, and a combination thereof.
[0054] In addition, the solid electrolyte layer may have a thickness of 0.5 μm to 85 mm. When the thickness is less than 0.5 μm, the solid electrolyte layer may be too thin to be etched in the focused ion device. When the thickness is greater than 85 mm, it may be difficult to place the solid electrolyte layer in the chamber of the focused ion device.
[0055] In addition, the lithium ion supply electrode can be used to analyze the lithium secondary battery material using at least one selected from the group consisting of a transmission electron microscope (TEM), a scanning electron microscope (SEM), an optical microscope (OM) and a scanning probe microscope (SPM) during the charging and discharging process of the lithium secondary battery. Preferably, the lithium ion supply electrode can be used to analyze the lithium secondary battery material using a transmission electron microscope (TEM) during the charging and discharging process of the lithium secondary battery.
[0056] 4 are images taken using a scanning electron microscope (SEM) in a focused ion beam apparatus, and the images show a process of manufacturing a lithium ion supplying electrode according to Example 1 using the focused ion beam apparatus.
[0057] Referring to Figure 4, the present invention provides a method for manufacturing a lithium ion supply electrode, the method comprising: (a) forming a liquid lithium layer on a solid electrolyte layer under inert gas conditions and at a temperature at or above the melting point of lithium, and forming a protective layer containing a metal on the liquid lithium layer, thereby preparing a laminated material including a solid electrolyte layer, a lithium layer and a protective layer; and (b) separating a portion of the laminated material using a focused ion beam device at a temperature below the melting point of lithium so that the separated portion has a predetermined shape, thereby producing a lithium ion supply electrode including a solid electrolyte layer, a lithium layer and a protective layer.
[0058] In addition, step (a) can be carried out at a temperature ranging from 180.5°C to 500°C, and preferably ranging from 200°C to 300°C. When the temperature is lower than 180.5°C, lithium does not become liquid, and thus a liquid lithium layer cannot be formed on the solid electrolyte layer. Therefore, a temperature lower than 180.5°C is undesirable. When the temperature is higher than 500°C, this is undesirable because the temperature has a structural effect on the protective layer or the solid electrolyte layer.
[0059] In the method, the steps may include: (a-1) wetting a solid electrolyte layer with liquid lithium to form a laminate of a solid electrolyte layer and a liquid lithium layer; and (a-2) placing a protective layer containing a metal on the liquid lithium layer to prepare a laminate of a solid electrolyte layer, a lithium layer and a protective layer.
[0060] Step (a) may further include step (a-1') performed between step (a-1) and step (a-2): (a-1') adjusting the thickness of the liquid lithium layer by adding liquid lithium to the liquid lithium layer or removing some liquid lithium from the liquid lithium layer at a temperature at or above the melting point of lithium.
[0061] In the method, step (b) may include: (b-1) using a focused ion beam device, etching a laminate material consisting of a solid electrolyte layer, a lithium layer and a protective layer into a bridge-shaped pattern when viewed from above the protective layer; (b-2) etching off one of the left and right ends of the bridge-shaped pattern and etching off the lower portion of the bridge-shaped pattern; (b-3) bonding a probe to the surface of the protective layer of the bridge-shaped pattern, etching the left or right end and the lower portion from the bridge-shaped pattern; and (b-4) etching off the remaining unetched ends of the left and right ends of the bridge-shaped pattern, thereby obtaining a lithium ion supply electrode comprising a protective layer, a lithium layer and a solid electrolyte layer and bonded to the probe.
[0062] The method may further include steps (c) and (d) performed after step (b-4): (c) bonding a protective layer and a lithium layer of a lithium ion supply electrode to the metal tip, but not bonding a portion or all of the solid electrolyte layer to the metal tip; and (d) etching the solid electrolyte layer so that a cross-sectional area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases.
[0063] The method may further include a step (c') performed before step (c): (c') bringing the lithium ion supply electrode bonded to the probe close to the metal tip, and rotating the probe so that the surface of the protective layer of the laminate material bonded to the probe, the surface of the lithium layer, and the surface of the solid electrolyte layer face the metal tip. Preferably, the surfaces of the protective layer, the lithium layer, and the solid electrolyte layer may each face the top side of the metal tip.
[0064] The present disclosure provides a method for real-time analysis of lithium secondary battery materials, the method comprising: (1) loading a lithium ion supply electrode into a first holder of a real-time bias holder; (2) loading a material for a lithium secondary battery into a second holder; and (3) bringing a solid electrolyte of the lithium ion supply electrode into contact with the material, and applying a voltage or current to the lithium ion supply electrode and the material to analyze the changes in the structure and interface of the material in real time using a microscope during charging or discharging.
[0065] In addition, the material for the lithium secondary battery may be any one selected from the group consisting of a negative electrode material, an electrolyte, a positive electrode material, and a current collector.
[0066] Furthermore, the microscope may be any one selected from the group consisting of a transmission electron microscope (TEM), a scanning electron microscope (SEM), an optical microscope (OM), and a scanning probe microscope (SPM), and may preferably be a transmission electron microscope (TEM).
[0067] The lithium ion supply electrode for real-time transmission electron microscopy analysis must be manufactured so that observation of structural defects and analysis of defect generation mechanisms can be performed by constructing a charging and discharging environment on a miniaturized scale. The lithium ion supply electrode must contain lithium and an electrolyte to supply lithium ions. During loading of the lithium ion supply electrode into the holder of the real-time transmission electron microscope, the lithium must not be oxidized but should be kept as it is.
[0068] To this end, three approaches were adopted.
[0069] The first approach is to minimize the lithium area exposed to air by wetting the solid electrolyte with liquid lithium in a glove box and by covering the solid electrolyte wetted by liquid lithium with a thin copper film that acts as a protective layer (see Figure 1 ) to prevent lithium oxidation. Since the water vapor partial pressure and oxygen partial pressure inside the glove box are strictly controlled, lithium will not be oxidized inside the glove box. In this step, since the thin copper film covering the lithium layer protects the lithium from the Ga ion beam while the etching process is performed with the focused ion beam device, the lithium ion supply electrode can be manufactured without depositing an additional protective layer.
[0070] The second way is to design a method for manufacturing a lithium ion supply electrode using a focused ion beam device. The use of the focused ion beam device enables observation by scanning electron microscopy, platinum (Pt) deposition, fine etching, and observation using a Ga ion beam to be performed simultaneously. Since the lithium ion supply electrode according to the present disclosure has a size of about 15×8×20 μm 3 However, by using a focused ion beam device, it is possible to manufacture a micro-sized lithium ion supply electrode and attach the manufactured electrode to a metal tip.
[0071] In the laminate composed of a solid electrolyte layer, a lithium layer and a protective layer produced by the first method, the protective layer to prevent oxidation of lithium is the top layer, and the solid electrolyte layer is the bottom layer. The thickness of the top layer is 6 μm, the thickness of the lithium layer directly below the top layer is about 5 μm, and the thickness of the solid electrolyte layer as the bottom layer is hundreds of μm or more. Since the focused ion beam device etches by emitting an ion beam that first impinges on the surface of the laminate and then diffuses into the laminate. Therefore, the laminate must be placed in the focused ion beam device with the protective layer of 6 μm facing upward, so that a sample including all of the solid electrolyte layer, the lithium layer and the protective layer can be produced (on the contrary, when the laminate is placed so that the solid electrolyte becomes the top layer, it is difficult to etch the laminate because the thickness of the solid electrolyte is hundreds of μm or more). When the electrode is separated from the laminate using a focused ion beam device, the protective layer is usually located at the top, and the lithium layer and the solid electrolyte layer are located below the protective layer in this order. However, when lithium ions are supplied to the lithium secondary battery material to be analyzed, the solid electrolyte layer capable of transporting lithium ions must be located at the top so that the lithium secondary battery material is in contact with the solid electrolyte layer. Therefore, in order to place the solid electrolyte layer at the top, the manufacturing method includes a process of rotating the probe by an angle of 180° using a focused ion beam device. Before the probe is rotated, the solid electrolyte is located at the bottom ( Figure 2a ), but after the probe is rotated 180°, the solid electrolyte is at the top ( Figure 2b ). Through this probe rotation method, a lithium-ion supply electrode can be manufactured in which a solid-state electrolyte is placed on top.
[0072] The third way is to control the thickness of the lithium layer to fall within the range of 0.5μm to 10μm when applying the first way. When the lithium layer is too thin (ie less than 0.5μm), not only is the lithium ion supply insufficient, but also a smooth interface will not be formed between the solid electrolyte layer and the lithium layer and between the lithium layer and the protective layer. In addition, there is a risk of air penetrating into the empty space and oxidizing the lithium. On the other hand, when the thickness of the lithium layer exceeds 10μm, it takes a long time to etch the lithium layer using a focused ion beam device, and the greater the etching amount, the more overused the focused ion beam device is. Therefore, the thickness of the lithium layer is optimized to be within the range of 0.5μm to 10μm. Embodiments of the invention
[0073] [Example]
[0074] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments are for illustrative purposes only, and the scope of the present invention is not limited thereto.
[0075] Example 1: Fabrication of a lithium ion supply electrode
[0076] The fabrication of the laminated material including the solid electrolyte layer, lithium layer and protective layer was carried out in a glove box with strictly controlled oxygen partial pressure and water vapor partial pressure. The lithium ribbon was melted using a hot plate heated to 260°C to prepare liquid lithium. The granular oxide-based solid electrolyte (Li7La3Zr2O 12 ) is wetted with liquid lithium to form a liquid layer. Next, the wetted lithium is reduced by two to three times so that the thickness of the lithium layer finally has a thickness of about 5 μm. A thin copper film with a thickness of 6 μm is placed on the lithium layer to form a laminate consisting of a solid electrolyte layer, a lithium layer and a protective layer. Next, the laminate is removed from the hot plate, fully cooled and sealed. After that, the sealed laminate is taken out of the glove box.
[0077] The sealed laminate was then unsealed and placed in a focused ion beam apparatus. The focused ion beam apparatus performs deposition, fine etching, and observation of platinum (Pt) by using a Ga ion beam. At this stage, an additional tungsten tip (manufacturer name: Probes, product name: WNP-10, tungsten nanoprobe) was installed so that it could be placed horizontally.
[0078] 4 is images taken using a scanning electron microscope (SEM) in a focused ion beam apparatus, and the images show a process of manufacturing a lithium ion supplying electrode according to Example 1 using the focused ion beam apparatus. Specifically, the images are taken using a scanning electron microscope, and the insets are taken using a focused ion beam apparatus.
[0079] Reference Figure 4a , by using a Ga ion beam with a voltage of 30 kV and a current of 21 nA, etching is performed on both sides of the laminated material including the solid electrolyte layer, the lithium layer and the protective layer to form a bridge pattern with a width ranging from 10 μm to 12 μm (when viewed along the z-axis direction). The etching area on each side of the bridge pattern is 30×30×25 μm 3 . Next, as shown in the inset, a focused ion device is used to check whether the interface layer between the protective layer and the lithium layer and the interface layer between the lithium layer and the solid electrolyte layer are formed, and whether the thickness of the lithium layer in the x-axis direction is qualified. When etching is performed at a high current, the etched surface is damaged. Therefore, with the applied voltage of 30 kV fixed, the applied current is first set to 9.3 nA, and then gradually reduced to 2.5 nA during the etching process, so that a smooth and well-trimmed etched surface can be obtained. At this stage, the width of the bridge pattern is adjusted to about 8 μm.
[0080] Reference Figure 4b, a light beam is emitted in the x direction to the cross section of the protective layer, the lithium layer and the solid electrolyte layer. By the light beam radiation, etching is performed in an L-shaped direction (when viewed in the x direction). That is, one of the left and right ends of the bridge pattern is etched away, and the lower part of the bridge pattern is etched away.
[0081] Next, refer to Figure 4c , inserting a probe and depositing platinum (Pt) to bond the probe to the upper surface of the protective layer on the pattern, and etching away one of the left and right ends and the lower portion from the pattern.
[0082] Reference Figure 4d , the remaining ends of the left and right ends of the pattern are etched so that the L-shaped etched portion is finally changed to form a U-shape. Thus, a lithium ion supply electrode including a protective layer, a lithium layer, and a solid electrolyte layer and bonded to a probe is manufactured.
[0083] Since the end of the metal tip has a size of several μm, which is smaller than the lithium ion supply electrode, the end of the metal tip is trimmed. Figure 4e , inserting the probe incorporating the lithium ion supply electrode into the trimmed end of the metal tip, and then Figure 4f FIG. 2 is a schematic diagram showing a lithium ion supply electrode before and after the probe is rotated 180° in a focused ion beam device. Referring to FIG. 2 and Figure 4f , before the probe is rotated, the protective layer, lithium layer, and solid electrolyte layer are arranged in this order from the top. However, when the probe is rotated 180°, the positions of the protective layer, lithium layer, and solid electrolyte layer change, so that the protective layer, lithium layer, and solid electrolyte layer are arranged in this order from the left to the right.
[0084] Reference Figure 4g , platinum is deposited to connect the protective layer and lithium layer of the lithium ion supply electrode to the end of the metal tip, and then the probe and the lithium ion supply electrode are separated from each other by etching.
[0085] Since the sample size of the transmission electron microscope is several micrometers, the surface of the lithium ion supply electrode needs to be processed to make it sharp. Figure 4h and Figure 4i , using a focused ion beam device to process the lithium-ion supply electrode into a surface morphology with a milk carton.
[0086] Example 2: Analysis of current collector of lithium secondary battery
[0087] In a real-time bias holder, the lithium ion supply electrode manufactured according to Example 1 is loaded into the first holder, the working electrode made of the current collector material is loaded into the second holder, and the solid electrolyte layer of the lithium ion supply electrode is brought into contact with the working electrode to form a half-cell consisting of a counter electrode (lithium layer of the lithium ion supply electrode), an electrolyte (solid electrolyte layer of the lithium ion supply electrode) and a working electrode (current collector material) arranged in the following order.
[0088] In this case, three different types of working electrodes were prepared: lithiophobic Cu, lithiophobic Ni, and lithiophobic Ni coated with lithiophilic Ag.
[0089] Herein, a lithiophobic material refers to a material that is not easily plated with pure lithium, and a lithiophilic material refers to a material that is easily plated with pure lithium.
[0090] Next, the half-cells were imaged in real time using a transmission electron microscope while the contacted half-cells were charged and discharged.
[0091] Comparative Example 1: Production of a lithium ion supply electrode without a protective layer
[0092] A lithium ion supplying electrode was manufactured in the same manner as in Example 1, except that a thin copper film having a thickness of 6 μm was not placed on the lithium layer.
[0093] [Experimental example]
[0094] Experimental Example 1: Evaluation of the Antioxidation Effect of the Lithium Protective Layer
[0095] 3 is images taken using a scanning electron microscope (SEM) in a focused ion beam apparatus, and these images show the degree of oxidation of lithium in each laminated material prepared according to Example 1 and Comparative Example 1. FIG.
[0096] Figure 3a is a SEM image of a cross section of a laminate of a solid electrolyte layer and a lithium layer according to Comparative Example 1. Specifically, Figure 3a is a SEM image taken after placing the solid electrolyte layer / lithium layer laminated material prepared according to Comparative Example 1 on a focused ion beam device. During the process of placing the laminated material on the focused ion beam device, the time period for which the laminated material is exposed to air is 5 minutes or less. Figure 3a , due to the absence of a protective layer (thin metal film), lithium is oxidized, making the interface layer between the lithium layer and the solid electrolyte layer not smooth.
[0097] Figure 3b : is a SEM image of a cross section of a structure in which platinum (Pt) is deposited on the surface of the solid electrolyte layer / lithium layer laminate of Comparative Example 1. In this case, the deposited platinum forms a protective layer to protect the sample from the Ga ion beam. Figure 3b, since the laminated material of the comparative example is not provided with a protective layer, the lithium is damaged during the deposition process and an empty space is formed in the interface between the lithium oxide layer and the deposited platinum layer.
[0098] Figure 3c is a SEM image of a cross section of a solid electrolyte layer / lithium layer / protective layer laminate when manufacturing a lithium ion supply electrode according to Example 1. Figure 3c In the case of Example 1, since the lithium in the lithium layer was not oxidized, no lithium oxide layer was formed. Therefore, it was confirmed that a smooth interface was formed between the lithium layer and the solid electrolyte layer.
[0099] Figure 3d is a SEM image of a cross section of the solid electrolyte layer / lithium layer / protective layer laminate of Example 1 taken after being stored in a vacuum desiccator for 7 days. Figure 3d , confirming that even after 7 days of storage, the laminate of Example 1 still maintains a smooth interface without lithium oxidation.
[0100] That is, in the case where the protective layer as a shield is not formed, lithium is oxidized even in a short period of 5 minutes or less when the laminate is loaded into the focused ion beam device. However, in the case where the protective layer is formed, lithium is not oxidized even after storage in a vacuum desiccator for 7 days.
[0101] Figure 3e The solid electrolyte layer / lithium layer / protective layer laminate of Example 1 is etched into a bridge pattern using a focused ion beam device, and then the etched pattern is exposed to air for 7 days, and the laminate is observed using a focused ion beam device. Figure 3e , it was confirmed that the lithium exposed to the air due to etching was oxidized, and thus the volume of the lithium layer increased. That is, even if a protective layer is formed, lithium oxidation will occur if the lithium layer is exposed to the air for a long time.
[0102] Figure 3f It shows the observation Figure 3e A view of the resulting interface around the area of the structure exposed to air. Figure 3f , based on the fact that the volume of the lithium layer increased and pores were formed, it was confirmed that the lithium layer was oxidized to a depth of 80 μm from the exposure point. On the other hand, Figure 3f The dotted square area in the figure is more than 80 μm away from the exposure point. Therefore, the dotted square area is not oxidized.
[0103] Therefore, in the case where the protective layer is formed as in the laminated material of Example 1, if a lithium ion supply electrode is manufactured in a region 80 μm from the air exposure point, a lithium ion supply electrode without lithium oxidation can be obtained although the lithium layer is exposed to the air.
[0104] Experimental Example 2: Evaluation of the performance of the lithium ion supply electrode
[0105] 5 is a diagram showing a process of loading the prepared lithium ion supplying electrode and the working electrode (current collector material) in a real-time bias holder for precipitation reaction analysis of a lithium secondary battery current collector according to Example 2. Based on the results of the precipitation reaction analysis of the working electrode, it can be evaluated whether the lithium ion supplying electrode according to the present disclosure works properly.
[0106] Figure 5a is a schematic diagram showing an analysis experiment of a current collector of a lithium secondary battery according to Example 2, Figure 5b is an image of a lithium ion supply electrode according to Example 1, and Figure 5c : is a diagram showing the state of the working electrode of Example 2 made of lithium-phobic Cu. Figure 5d It is an image of a real-time bias holder when the lithium ion supply electrode and the working electrode (lithium-phobic Cu) prepared according to Example 1 are loaded for the current collector analysis experiment of the lithium secondary battery according to Example 2, and a low-magnification TEM image of the bias holder mounted on a transmission electron microscope.
[0107] 6 is a view showing the experimental results of Example 2 when using lithium-phobic Cu as a working electrode. Specifically, Figure 6a is a TEM image of the interface between the lithium ion supply electrode of Example 1 and the lithium-phobic Cu electrode in an environment where a constant current of +10uA or -10uA is applied, and Figure 6b TEM images of the interface between the lithium ion supply electrode of Example 1 and the lithium-phobic Cu electrode in an environment where a constant current of +20 uA or -20 uA is applied.
[0108] Reference Figure 6a and Figure 6b , when a positive current of +10uA or +20uA is applied, a precipitation reaction occurs at the interface between the lithium ion supply electrode and the working electrode (Cu, lithium-phobic material), and lithium particles grow. The lithium particles grow larger at a relatively high current of +20uA. When a negative current of -10uA or -20uA is applied, lithium ions move from the interface to the lithium ion supply electrode, thereby reducing the size of the lithium particles.
[0109] 7 is a diagram showing the experimental results of Example 2 when using lithium-phobic Ni as a working electrode. Specifically, Figure 7a is a TEM image of the interface between the lithium ion supply electrode and the working electrode (lithium-phobic Ni) of Example 1 in an environment where a constant current of +8 pA is applied, and Figure 7bis a TEM image of the interface between the lithium ion supply electrode and the working electrode (lithium-phobic Ni) of Example 1 in an environment where a constant current of -8 pA is applied.
[0110] Reference Figure 7a , when a current of +8 pA was applied, a precipitation reaction occurred at the interface between the lithium ion supply electrode and the working electrode (Ni, lithium-phobic material), and the lithium particles became dendrites.
[0111] Reference Figure 7b , when a current of −8 pA was applied, lithium ions moved toward the lithium ion supply electrode and thus the size of lithium grown at the interface decreased.
[0112] FIG. 8 is a graph showing the experimental results of Example 2 when lithiophobic Ni coated with lithiophilic Ag is used as a working electrode.
[0113] Specifically, Figure 8a is a low-magnification TEM image of the interface between the lithium ion supply electrode and the working electrode (lithophobic Ni coated with lithiophilic Ag) of Example 1 in a state where charging and discharging are not performed, and Figure 8b is a low-magnification TEM image of the interface between the lithium ion supply electrode and the working electrode (lithophobic Ni coated with lithiophilic Ag) of Example 1 in an environment where a constant current of +20 nA is applied.
[0114] Figure 8c High-magnification TEM images of the interface between the lithiophilic Ag and the lithiophobic Ni of the working electrode in Example 1 are shown, and these images were taken under the conditions of pre-bias, constant current (bias) of +20nA, and constant current (bias) of -20nA, respectively.
[0115] Figure 8d High-magnification TEM images of the interface between the lithiophilic Ag and the lithiophobic Ni of the working electrode in Example 1 are shown, which were taken under the conditions of pre-bias, constant current (bias) of +160nA, and constant current (bias) of -160nA, respectively.
[0116] Reference Figure 8a , in the working electrode, the lithium-philic Ag coating layer has a thickness in the range of 150 nm to 200 nm and is formed on the lithium-phobic material Ni.
[0117] Reference Figure 8b , in a low-magnification observation environment, it was found that there were no lithium particles in the interface between the lithium-ion supply electrode and the working electrode (lithium-phobic Ni coated with lithiophilic Ag), and that a slight change occurred in the interface when a current of +20 nA was applied.
[0118] On the other hand, refer to Figure 8c , under an applied current of +20 nA or in a high-magnification observation environment, the black pattern indicated by the white arrow appears in a +20 nA constant current environment (bias: +20 nA) and disappears in a -20 nA constant current environment (bias: -20 nA).
[0119] In addition, refer to Figure 8d , in the Figure 8c Compared to the relatively high current environment (bias: +160nA), the size of the black pattern is larger than Figure 8c This change indicates that the lithiophilic material coating (Ag) leads to the lithiation and delithiation of the lithiophobic material (Ni).
[0120] That is, when the lithium ion supply electrode according to the present disclosure is used, not only the lithium precipitation process but also the lithiation / delithiation reaction of the lithium-phobic material can be observed.
[0121] Therefore, when the lithium ion supply electrode according to the present disclosure is used, it is possible to observe the lithium growth morphology in various micro-current and voltage environments and analyze the changes in the structure and interface of various lithium-phobic / lithiophilic materials of secondary battery materials in real time.
[0122] 9 is a view showing lithium particles generated during the precipitation reaction analysis of Example 2 when lithium-phobic Cu is used as a working electrode, and showing a change in shape of a lithium ion supplying electrode when the electrode is exposed to air after the analysis.
[0123] Specifically, in the case of using Cu as a lithium-phobic material during the experiment of Example 2, Figure 9a A high-resolution transmission electron microscope (HRTEM) image (upper left) and a fast Fourier transform (FFT) image (lower left) of lithium oxide (Li2O) are shown, and a high-resolution transmission electron microscope (HRTEM) image (upper right) and an FFT image (lower right) of lithium (Li) are shown. Since the growing lithium particles are susceptible to the high-intensity electron beam, the changes in the diffraction pattern are observed by irradiating the growing lithium particles with a high-intensity electron beam.
[0124] Reference Figure 9a , confirming that the particles grown at the interface between the lithium ion supplying electrode prepared according to Example 1 and the working electrode (Cu, lithium-phobic material) are lithium.
[0125] Figure 9b is an image taken immediately after the production of the lithium ion supply electrode of Example 1 before the precipitation reaction analysis of Example 2, and Fig.9c This is an image taken after the lithium ion supply electrode of Example 1 was exposed to air for seven days after the precipitation reaction analysis of Example 2.
[0126] Reference Figure 9b and Fig.9c , it was observed that the lithium in the lithium ion supply electrode was oxidized by exposure to air for one week to produce lithium oxide. The lithium ion supply electrode was covered with lithium oxide. Through this experiment, it was confirmed that lithium existed in the lithium ion supply electrode as lithium metal during the experiment.
[0127] The scope of the present invention is defined by the claims rather than the detailed description above, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be construed as falling within the protection scope of the present invention. Industrial Applicability
[0128] The lithium ion supply electrode disclosed herein is used for real-time analysis of lithium secondary battery materials in a charging and discharging environment. For this purpose, the lithium ion supply electrode uses a solid electrolyte with high lithium ion conductivity. In addition, the lithium ion supply electrode disclosed herein has the effect of maintaining the amount of lithium by preventing lithium oxidation when the electrode is loaded into a holder.
[0129] In addition, since the lithium ion supply electrode of the present invention has the advantage of preventing lithium oxidation in a short time, a glove box is not required. Therefore, the lithium ion supply electrode of the present invention can be used for the analysis of structural changes and interface responses of lithium secondary battery materials using equipment sensitive to light and vibration (e.g., transmission electron microscope).
Claims
1. A lithium ion supply electrode, comprising: a solid electrolyte layer, the solid electrolyte layer comprising a solid electrolyte; a lithium layer formed on the solid electrolyte layer and comprising lithium; as well as A protective layer is formed on the lithium layer and includes a metal.
2. The lithium ion supply electrode according to claim 1, wherein The lithium layer has a thickness of 0.5 μm to 10 μm.
3. The lithium ion supply electrode according to claim 1, wherein The metal in the protective layer includes one or more metals selected from the group consisting of copper (Cu), gold (Au), silver (Ag), and nickel (Ni).
4. The lithium ion supply electrode according to claim 3, wherein: The metal in the protection layer includes copper (Cu).
5. The lithium ion supply electrode according to claim 1, wherein The protective layer has a thickness of 0.5 μm to 10 μm.
6. The lithium ion supply electrode according to claim 1, wherein The cross-sectional area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases.
7. The lithium ion supply electrode according to claim 1, wherein The solid electrolyte layer has any one shape selected from the group consisting of a circular cone shape, an elliptical cone shape, and a polygonal pyramid shape.
8. The lithium ion supply electrode according to claim 1, wherein The solid electrolyte includes one or more selected from the group consisting of oxide-based solid electrolytes, sulfide-based solid electrolytes, phosphide-based solid electrolytes, silicide-based solid electrolytes and combinations thereof.
9. The lithium ion supply electrode according to claim 1, wherein: The solid electrolyte layer has a thickness of 0.5 μm to 85 mm.
10. The lithium ion supply electrode according to claim 1, wherein The lithium ion supply electrode is used to analyze lithium secondary battery materials during charging and discharging of the lithium secondary battery using any one selected from the group consisting of a transmission electron microscope, a scanning electron microscope, an optical microscope, and a scanning probe microscope.
11. A method for manufacturing a lithium ion supply electrode, the method comprising: (a) forming a liquid lithium layer on a solid electrolyte layer under an inert gas condition at a temperature at or above the melting point of lithium, and forming a protective layer comprising a metal on the liquid lithium layer, thereby obtaining a laminated material comprising the solid electrolyte layer, the lithium layer and the protective layer; as well as (b) separating a portion of the laminated material into a predetermined shape using a focused ion beam device at a temperature below the melting point of lithium, thereby producing a lithium ion supplying electrode including the solid electrolyte layer, the lithium layer and the protective layer.
12. The method according to claim 11, wherein: The step (a) is performed at a temperature ranging from 180.5°C to 500°C.
13. The method according to claim 11, wherein: The step (a) comprises: (a-1) wetting the solid electrolyte with liquid lithium to form a laminate of the solid electrolyte layer and the liquid lithium layer; and (a-2) placing the protective layer comprising a metal on the liquid-phase lithium layer to prepare a laminate of the solid electrolyte layer, the lithium layer and the protective layer.
14. The method according to claim 13, wherein: The step (a) further comprises (a-1') between the step (a-1) and the step (a-2): (a-1′) adjusting the thickness of the liquid lithium layer by adding liquid lithium to the liquid lithium layer or removing some liquid lithium from the liquid lithium layer at a temperature at or above the melting point of lithium.
15. The method according to claim 11, wherein: The step (b) comprises: (b-1) using a focused ion beam device, etching the laminated material consisting of the solid electrolyte layer, the lithium layer and the protective layer to obtain a bridge-shaped pattern when viewed from above the protective layer; (b-2) etching either the left end or the right end of the bridge pattern; (b-3) binding a probe to the surface of the protective layer in the bridge-shaped pattern; and (b-4) etching the remaining unetched ends of the left and right ends of the bridge pattern, thereby obtaining a lithium ion supply electrode including the protective layer, the lithium layer, and the solid electrolyte layer and bonded to the probe.
16. The method according to claim 15, further comprising: (c) bonding the protective layer and the lithium layer of the lithium ion supply electrode to a metal tip, but not bonding a part or all of the solid electrolyte layer to the metal tip; as well as (d) etching the solid electrolyte layer of the lithium ion supply electrode so that the cross-sectional area of the solid electrolyte layer parallel to the lithium layer decreases as the distance from the lithium layer increases, Wherein, step (c) and step (d) are performed after step (b-4).
17. The method according to claim 16, further comprising: (c') bringing the lithium ion supply electrode bonded to the probe close to the metal tip, and rotating the probe so that the surface of the protective layer, the surface of the lithium layer, and the surface of the solid electrolyte layer of the protective layer / lithium layer / solid electrolyte layer laminate material bonded to the probe face the metal tip, Wherein, step (c') is performed before step (c).
18. A method for real-time analysis of lithium secondary battery materials, the method comprising: (1) loading the lithium ion supply electrode according to claim 1 into a first holder; (2) loading a material for a lithium secondary battery into the second holder; as well as (3) bringing the solid electrolyte of the lithium ion supply electrode into contact with the material, applying voltage or current to the lithium ion supply electrode and the material, and observing changes in the structure and interface of the material in real time using a microscope during charging or discharging.
19. The method according to claim 18, wherein: The material for the lithium secondary battery is any one selected from the group consisting of a negative electrode material, an electrolyte, a positive electrode material and a current collector.
20. The method according to claim 18, wherein: The microscope is any one selected from the group consisting of a transmission electron microscope, a scanning electron microscope, an optical microscope and a scanning probe microscope.