Positive photosensitive resin composition, cured product, organic el display device, and method for producing cured product

By using a specific combination of photosensitive resin compositions in an organic EL display device, the problem of performance degradation of materials under high temperature, high humidity and light irradiation conditions in the prior art is solved, and high sensitivity, good development adhesion, and Heat resistance and bending resistance improve the reliability of the display device.

CN118749088APending Publication Date: 2024-10-08TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023538.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-22
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to develop photosensitive resin compositions with high sensitivity, good development adhesion, high heat resistance and bending resistance with the existing technology. Especially in organic EL display devices with high reliability requirements, existing materials have high temperature resistance. , high humidity and light exposure conditions show problems of reduced luminous brightness and pixel shrinkage.

Method used

A positive photosensitive resin composition containing free polyimide, polybenzoxazole, polyhydroxystyrene, quinonediazide compound and polar aprotic solvent is used to generate acid by adjusting the component ratio and adding thermal acid agent to improve the cured properties of the resin.

Benefits of technology

It achieves high sensitivity, good development adhesion, heat resistance and bending resistance, improving the reliability and performance stability of organic EL display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008393080000081
    Figure BDA0005008393080000081
  • Figure BDA0005008393080000111
    Figure BDA0005008393080000111
  • Figure BDA0005008393080000121
    Figure BDA0005008393080000121
Patent Text Reader

Abstract

The purpose of the present invention is to provide a positive photosensitive resin composition which has high sensitivity, good development adhesion, high heat resistance, high bending resistance of a cured product, and high reliability when the cured product is used in an organic EL display device. The present invention is a positive photosensitive resin composition containing: (A) one or more substances selected from the group consisting of polyimides, polyimide precursors, and copolymers thereof; (B) one or more compounds selected from the group consisting of polybenzoxazoles, polybenzoxazole precursors, and copolymers thereof; (C) polyhydroxystyrene, and / or a copolymer of polyhydroxystyrene and polystyrene; (D) a quinonediazide compound; and (E) a solvent, the content of the component (B) being 10-100 parts by mass per 100 parts by mass of the component (A), and the content of the component (C) being 1-90 parts by mass per 100 parts by mass of the component (A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive photosensitive resin composition, a cured product using the same, an organic EL display device having the cured product, and a method for producing the cured product. Background Art

[0002] Many products using organic electroluminescent (hereinafter referred to as “organic EL”) display devices have been developed for display devices having thin displays such as smartphones, tablet computers, and televisions.

[0003] Typically, an organic EL display device has a driving circuit, a planarization layer, a first electrode, a pixel segmentation layer, a light-emitting layer, and a second electrode on a substrate, and can emit light by applying a voltage between the opposing first electrode and the second electrode, or by passing a current. Among them, as a material for a planarization layer and a material for a pixel segmentation layer, a photosensitive resin composition that can be patterned by ultraviolet irradiation is generally used. Among them, in the case of a photosensitive resin composition using a polyimide resin, since the resin has high heat resistance, the gas component generated by the cured product obtained by low-temperature curing at about 200 to 270°C is small, so a highly reliable organic EL display device can be obtained, and from this point of view, it is preferably used (for example, see patent document 1).

[0004] On the other hand, the requirements for high reliability of organic EL display devices are becoming more stringent year by year, and for planarization layer materials and pixel segmentation layer materials, high reliability materials are also required that do not cause a decrease in luminous brightness or pixel shrinkage even after reliability tests under accelerated conditions such as high temperature, high humidity, and light irradiation. Here, pixel shrinkage refers to the phenomenon that the luminous brightness decreases from the end of the pixel or becomes dim.

[0005] In addition, photosensitive resin compositions are required to have higher sensitivity in order to shorten exposure time due to reasons such as increasing the size of substrates and improving productivity. On the other hand, highly sensitive materials have a problem of poor development adhesion, and photosensitive resin compositions are required to have better development adhesion.

[0006] In recent years, the development of flexible organic EL display devices formed on resin film substrates has been actively carried out. The flexible organic EL display device has a bendable portion and / or a portion fixed in a bent state in structure, and bending stress is applied to the planarization layer and the pixel division layer in the bent portion. In a flexible organic EL display device including such a bent portion, high bending resistance is required for the material for the planarization layer and the material for the pixel division layer.

[0007] Under such background, there is a strong demand for the development of a photosensitive resin composition that can be patterned with high sensitivity and can provide a cured product having high heat resistance and flex resistance and excellent reliability.

[0008] In response to such a problem, siloxane resins have been studied as photosensitive resin compositions that can achieve high sensitivity (for example, see Patent Document 2). In addition, as photosensitive resin compositions that can impart high bending resistance, the addition of specific phenolic hydroxyl-containing compounds and phenolic antioxidants to photosensitive resin compositions has been studied (for example, see Patent Document 3).

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2002-91343

[0012] Patent Document 2: Japanese Patent Application Publication No. 2006-178436

[0013] Patent Document 3: International Publication No. 2019-065351 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, it is difficult to say that the materials proposed in the above-listed patent documents have sufficient performance for applications requiring higher reliability, such as vehicle-mounted displays. In view of the above problems, the present invention aims to provide a photosensitive resin composition having high sensitivity, good development adhesion, high heat resistance, high bending resistance of the cured product, and high reliability when the cured product is used in an organic EL display device.

[0016] Means for solving problems

[0017] The present invention is as follows.

[0018] [1] A positive photosensitive resin composition comprising: (A) one or more selected from the group consisting of polyimide, polyimide precursor and copolymers thereof; (B) one or more selected from the group consisting of polybenzoxazole, polybenzoxazole precursor and copolymers thereof; (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene; (D) a quinonediazide compound; and (E) a solvent.

[0019] The content of the component (B) is 10 to 100 parts by mass based on 100 parts by mass of the component (A).

[0020] The content of the component (C) is 1 to 90 parts by mass based on 100 parts by mass of the component (A).

[0021] [2] The positive photosensitive resin composition according to [1], wherein, when the content of the component (A) is [PI] (mass), the content of the component (B) is [PB] (mass), and the content of the component (C) is [PH] (mass),

[0022] The mass ratio [PI] / ([PB]+[PH]) is in the range of 0.5≤[PI] / ([PB]+[PH])≤5.0.

[0023] [3] The positive photosensitive resin composition according to [2], wherein the relationship between [PB] and [PH] is [PB]>[PH].

[0024] [4] The positive photosensitive resin composition according to [3], wherein the mass ratio of [PB] to [PH] is in the range of 1.01≤[PB] / [PH]≤55.00.

[0025] [5] The positive photosensitive resin composition according to any one of [1] to [4], wherein the component (C) contains polyhydroxystyrene.

[0026] [6] The positive photosensitive resin composition according to any one of [1] to [5], wherein the solvent (E) contains a polar aprotic solvent.

[0027] [7] The positive photosensitive resin composition according to [6], wherein the content of the polar aprotic solvent is 1 to 30% by mass relative to 100% by mass of the solvent (E).

[0028] [8] The positive photosensitive resin composition according to any one of [1] to [7], wherein the solid content concentration of the positive photosensitive resin composition is 3 to 30% by mass.

[0029] [9] The positive photosensitive resin composition according to any one of [1] to [8], wherein the component (B) comprises a resin having a structural unit represented by the formula (1) described below as a main chain.

[0030]

[10] The positive photosensitive resin composition according to any one of [1] to [9], further comprising (F) a thermal acid generator.

[0031]

[11] The positive photosensitive resin composition according to

[10] , wherein the thermal acid generator (F) contains a thermal acid generator having a sulfonate structure.

[0032]

[12] The photosensitive resin composition according to

[10] or

[11] , wherein the thermal acid generator (F) contains a compound represented by the formula (2) described below.

[0033]

[13] A cured product obtained by curing the positive photosensitive resin composition according to any one of [1] to

[12] .

[0034]

[14] A solidified material, wherein, when analyzed by reaction pyrolysis GC / MS, a compound represented by formula (3) described later, a compound represented by formula (4) described later, and a compound represented by formula (5) described later are detected, and in terms of the detection peak intensity ratio, when the compound represented by formula (4) is set to 1, the compound represented by formula (3) is 0.1 to 1, and the compound represented by formula (5) is 0.1 to 3.

[0035]

[15] An organic EL display device comprising the cured product according to

[13] or

[14] .

[0036]

[16] A method for producing a cured product, the method comprising the following steps in sequence: (1) applying the positive photosensitive resin composition described in any one of [1] to

[12] to a substrate to form a positive photosensitive resin film; (2) drying the positive photosensitive resin film; (3) exposing the dried positive photosensitive resin film through a photomask; (4) developing the exposed positive photosensitive resin film; and (5) heating the developed positive photosensitive resin film.

[0037] Effects of the Invention

[0038] The photosensitive resin composition of the present invention can provide a photosensitive resin composition having high sensitivity, good development adhesion, high heat resistance, high bending resistance of a cured product, and high reliability when the cured product is used in an organic EL display device. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] [ Figure 1 ] is a cross-sectional view of an organic EL display device in which a planarization layer and a pixel division layer are formed.

[0040] [ Figure 2 ] is a schematic diagram of a substrate of an organic EL display device. DETAILED DESCRIPTION

[0041] Embodiments of the present invention will be described in detail.

[0042] The positive photosensitive resin composition of the present invention is the following positive photosensitive resin composition, which contains: (A) one or more selected from the group consisting of polyimide, polyimide precursor and copolymers thereof (hereinafter, sometimes referred to as (A) component); (B) one or more selected from the group consisting of polybenzoxazole, polybenzoxazole precursor and copolymers thereof (hereinafter, sometimes referred to as (B) component); (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene (hereinafter, sometimes referred to as (C) component); (D) a quinonediazide compound; and (E) a solvent.

[0043] The content of the component (B) is 10 to 100 parts by mass based on 100 parts by mass of the component (A).

[0044] The content of the component (C) is 1 to 90 parts by mass based on 100 parts by mass of the component (A).

[0045] By making the content of component (B) 10 to 100 parts by mass relative to 100 parts by mass of the aforementioned component (A), a cured product with good heat resistance and bending resistance can be obtained. By making the content of component (C) 1 to 90 parts by mass relative to 100 parts by mass of the aforementioned component (A), the sensitivity of the resin composition is improved and the development adhesion becomes good. By containing the three components (A) to (C), a photosensitive resin composition with high sensitivity, good development adhesion, high heat resistance, high bending resistance of the cured product, and high reliability when the cured product is used in an organic EL display device can be provided.

[0046] The positive photosensitive resin composition of the present invention contains (A) one or more selected from the group consisting of polyimide, polyimide precursor, and copolymers thereof.

[0047] (A) Component may contain a known polyimide including a structural unit of a polyimide, a known polyimide precursor including a structural unit of a polyimide precursor, and a known copolymer thereof. In the present invention, (A) Component is defined as a resin having an imide bond in the main chain.

[0048] In addition, when (A) component contains the structural unit of a polyimide and / or the structural unit of a polyimide precursor, and the structural unit of a polybenzoxazole and / or the structural unit of a polybenzoxazole precursor, it is described as (A) component.

[0049] The component (A) preferably has an alkali-soluble group. Alkali solubility means that: a solution obtained by dissolving a resin in γ-butyrolactone is applied to a silicon wafer, and pre-baked at 120° C. for 4 minutes to form a pre-baked film with a film thickness of 10 μm±0.5 μm, and the pre-baked film is immersed in a 2.38 mass % tetramethylammonium hydroxide aqueous solution at 23±1° C. for 1 minute, and then rinsed with pure water, and the dissolution rate obtained based on the reduction in film thickness at this time is 50 nm / minute or more.

[0050] In order to impart alkali solubility, it is preferred that an acidic group is present in the structural unit of the resin and / or at the end of its main chain. As the acidic group, for example, a carboxyl group, a phenolic hydroxyl group, a sulfonic acid group, a thiol group, etc. can be cited. In addition, component (A) preferably has a fluorine atom, which imparts hydrophobicity to the interface between the film and the substrate when developing with an alkaline aqueous solution, and can inhibit the penetration of the alkaline aqueous solution into the interface. With regard to the fluorine atom content of component (A), from the viewpoint of preventing the penetration of the alkaline aqueous solution into the interface, it is preferably more than 5% by mass, and from the aspect of solubility in the alkaline aqueous solution, it is preferably less than 20% by mass.

[0051] The component (A) can be synthesized by a known method.

[0052] In the case of a polyimide precursor, if it is a polyamic acid, it can be synthesized by, for example, a method of reacting tetracarboxylic dianhydride with a diamine compound at low temperature. If it is a polyamic acid ester, it can be synthesized by, for example, the following methods: a method of reacting tetracarboxylic dianhydride with a diamine compound at low temperature, and then partially esterifying the amic acid structure using N,N-dimethylformamide dimethyl acetal or the like; a method of obtaining a diester using tetracarboxylic dianhydride and an alcohol, and then reacting in the presence of an amine and a condensing agent; a method of obtaining a diester using tetracarboxylic dianhydride and an alcohol, and then chlorinating the remaining dicarboxylic acid to react it with an amine; and the like.

[0053] In the case of polyimide, it can be obtained, for example, by dehydrating and ring-closing the polyamic acid or polyamic acid ester obtained by the above method by heating or chemical treatment with an acid, an alkali or the like in a solvent.

[0054] Specific examples of the tetracarboxylic dianhydride used in the component (A) include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)ethane dianhydride, and bis(3,4-dicarboxyphenyl)ethane dianhydride. Aliphatic tetracarboxylic acid dianhydrides such as bis(4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, 1,2,5,6-naphthalenetetracarboxylic acid dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 2,3,5,6-pyridinetetracarboxylic acid dianhydride, 3,4,9,10-perylenetetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, butanetetracarboxylic acid dianhydride, and 1,2,3,4-cyclopentanetetracarboxylic acid dianhydride may be used as the tetracarboxylic acid dianhydride used as the component (A). Two or more of these may be used.

[0055] Specific examples of the diamine compound used in the component (A) include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4 '-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene or a compound obtained by replacing at least a part of hydrogen atoms of the aromatic ring thereof with an alkyl group or a halogen atom, aliphatic cyclohexyldiamine, methylenebiscyclohexylamine and diamines of the structures shown below. Two or more of these can be used as the diamine compound.

[0056] [Chemical formula 1]

[0057]

[0058] R 3 and R 6 Each independently represents an oxygen atom, C(CF3)2 or C(CH3)2. 4 , R 5 and R 7 ~R 14 Each independently represents a hydrogen atom or a hydroxyl group.

[0059] In order to improve the storage stability of the positive photosensitive resin composition, the main chain terminals of the components (A) are preferably blocked with known end-blocking agents such as monoamines, acid anhydrides, monocarboxylic acids, monoacyl chloride compounds, and monoactive ester compounds. For the purpose of improving the chemical resistance of the cured resin obtained by calcination, monoamines, acid anhydrides, monocarboxylic acids, monoacyl chloride compounds, and monoactive ester compounds having at least one alkenyl or alkynyl group may be used as these end-blocking agents.

[0060] About the content of the end-capping agent such as monoamine, anhydride, acyl chloride, monocarboxylic acid, from the viewpoint of improving storage stability, relative to the sum 100 mol % of all monomer components constituting (A) component, preferably more than 1 mol %, more preferably more than 5 mol %. In addition, from the viewpoint of the resin that can obtain good film properties, relative to the sum 100 mol % of all monomer components constituting (A) component, preferably less than 40 mol %, more preferably less than 30 mol %. It is also possible to introduce a variety of different terminal groups in (A) component by reacting a variety of end-capping agents.

[0061] The positive photosensitive resin composition of the present invention contains (B) one or more selected from the group consisting of polybenzoxazole, polybenzoxazole precursor and copolymers thereof. In the present invention, the component (B) is defined as a resin having no imide bond in the main chain.

[0062] The component (B) may contain a known polybenzoxazole including a structural unit of polybenzoxazole, a known polybenzoxazole precursor including a structural unit of a polybenzoxazole precursor, and a known copolymer thereof.

[0063] In the present invention, component (B) preferably has an alkali-soluble group. In order to impart alkali solubility, it is preferred that the structural unit of component (B) and / or its main chain end have an acidic group. As the acidic group, for example, a carboxyl group, a phenolic hydroxyl group, a sulfonic acid group, a thiol group, etc. can be cited. In addition, component (B) preferably has a fluorine atom, which imparts hydrophobicity to the interface between the film and the substrate when developing with an alkaline aqueous solution, and can inhibit the penetration of the alkaline aqueous solution into the interface. With regard to the fluorine atom content in component (B), from the viewpoint of the effect of preventing the penetration of the alkaline aqueous solution into the interface, it is preferably 5% by mass or more, and from the aspect of solubility in an alkaline aqueous solution, it is preferably 20% by mass or less.

[0064] The component (B) can be synthesized by a known method.

[0065] In the case of a polybenzoxazole precursor, as a production method, a bisaminophenol compound can be obtained by condensing a dicarboxylic acid. Specifically, there are the following methods: a method of reacting a dehydration condensation agent such as dicyclohexylcarbodiimide (DCC) with an acid and adding a bisaminophenol compound thereto; a method of dripping a solution of dicarbonyl chloride into a solution of a bisaminophenol compound to which a tertiary amine such as pyridine is added; and the like.

[0066] In the case of polybenzoxazole, it can be obtained, for example, by subjecting the polybenzoxazole precursor obtained by the above method to dehydration ring closure in a solvent by heating or chemical treatment with an acid, an alkali or the like.

[0067] Examples of dicarboxylic acids used in the component (B) include terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, and triphenyl dicarboxylic acid. Examples of tricarboxylic acids include trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl trimaric acid. Examples of tetracarboxylic acids include pyromellitic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, 2,3,3',4'-biphenyl tetracarboxylic acid, 2,2',3,3'-biphenyl tetracarboxylic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, and 2,2',3,3'-diphenyl tetracarboxylic acid. Aliphatic tetracarboxylic acids such as ketotetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, butanetetracarboxylic acid, and 1,2,3,4-cyclopentanetetracarboxylic acid may be used. Two or more of these dicarboxylic acids used in the component (B) may be used.

[0068] Specific examples of the bisaminophenol compound used in the component (B) include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4, 4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene or a compound obtained by replacing at least a part of hydrogen atoms of the aromatic ring thereof with an alkyl group or a halogen atom, aliphatic cyclohexyldiamine, methylenebiscyclohexylamine and diamines of the structure shown below. Two or more of the bisaminophenol compounds used in the component (B) may be used.

[0069] [Chemical formula 2]

[0070]

[0071] R 3 and R 6 Each independently represents an oxygen atom, C(CF3)2 or C(CH3)2. 4 , R 5 and R 7 ~R 14 Each independently represents a hydrogen atom or a hydroxyl group.

[0072] In order to improve the storage stability of the positive photosensitive resin composition, the main chain terminals of the components (B) are preferably blocked with known end-blocking agents such as monoamines, acid anhydrides, monocarboxylic acids, monoacyl chloride compounds, and monoactive ester compounds. For the purpose of improving the chemical resistance of the cured resin obtained by calcination, monoamines, acid anhydrides, monocarboxylic acids, monoacyl chloride compounds, and monoactive ester compounds having at least one alkenyl or alkynyl group may be used as these end-blocking agents.

[0073] About the content of the end-capping agent such as monoamine, anhydride, acyl chloride, monocarboxylic acid, from the viewpoint of improving storage stability, relative to the sum 100 mol % of all monomer components constituting (B) component, preferably more than 1 mol %, more preferably more than 5 mol %. In addition, from the viewpoint of the resin that can obtain good film properties, relative to the sum 100 mol % of all monomer components constituting (B) component, preferably less than 40 mol %, more preferably less than 30 mol %. It is also possible to introduce a variety of different terminal groups in (B) component by reacting a variety of end-capping agents.

[0074] The content of the component (B) of the positive photosensitive resin composition is 10 to 100 parts by mass relative to 100 parts by mass of the aforementioned component (A). If the content of the component (B) is less than 10 parts by mass relative to 100 parts by mass of the aforementioned component (A), the bending resistance is reduced. The content of the component (B) is preferably 20 parts by mass or more. On the other hand, if the content of the component (B) is greater than 100 parts by mass relative to 100 parts by mass of the aforementioned component (A), the heat resistance is reduced. The content of the component (B) is preferably 95 parts by mass or less relative to 100 parts by mass of the aforementioned component (A).

[0075] The component (B) preferably contains a resin having a structural unit represented by formula (1) as a main chain. By containing a resin having a structural unit represented by formula (1) as a main chain, the bending resistance is improved.

[0076] [Chemical formula 3]

[0077]

[0078] In formula (1), R 1 and R 2 Each independently represents a divalent to octavalent organic group having 2 to 30 carbon atoms. p represents an integer of 0 to 4, and q represents an integer of 1 to 4.

[0079] The positive photosensitive resin composition of the present invention contains (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene.

[0080] The term "containing (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene" means containing either or both of polyhydroxystyrene and a copolymer of polyhydroxystyrene and polystyrene.

[0081] The component (C) of the present invention can be synthesized by a known method.

[0082] As the manufacturing method of (C) component, the phenol derivative with unsaturated bond can be obtained by addition polymerization. As the phenol derivative with unsaturated bond, for example, hydroxystyrene, dihydroxystyrene, allylphenol, coumaric acid, 2'-hydroxychalcone, N-hydroxyphenyl-5-norbornene-2,3-dicarboximide, resveratrol 4-hydroxystilbene, etc. can be cited, and two or more of them can be used. In addition, it can also be a copolymer formed with monomers such as styrene that do not contain phenolic hydroxyl groups. In this way, the adjustment of the alkali dissolution rate of (C) component becomes easy.

[0083] The content of component (C) is 1 to 90 parts by mass relative to 100 parts by mass of component (A). If the content of component (C) is less than 1 part by mass relative to 100 parts by mass of component (A), the sensitivity decreases. The content of component (C) is preferably 3 parts by mass or more relative to 100 parts by mass of component (A). On the other hand, if the content of component (C) is greater than 90 parts by mass relative to 100 parts by mass of component (A), the development adhesion decreases. The content of component (C) is preferably 70 parts by mass or less relative to 100 parts by mass of component (A).

[0084] The preferred weight average molecular weight of component (C) can be determined by gel permeation chromatography (GPC) in terms of polystyrene. From the viewpoint of sensitivity, it is preferably 1000 or more, more preferably 3000 or more, and further preferably 4000 or more. From the viewpoint of development adhesion, it is preferably 10000 or less, more preferably 8000 or less, and further preferably 7000 or less.

[0085] From the viewpoint of sensitivity, the component (C) preferably contains polyhydroxystyrene.

[0086] In the positive photosensitive resin composition of the present invention, when the content of the aforementioned component (A) is set to [PI] (mass), the content of the aforementioned component (B) is set to [PB] (mass), and the content of the aforementioned component (C) is set to [PH] (mass), the range of the mass ratio [PI] / ([PB]+[PH]) is preferably 0.5≤[PI] / ([PB]+[PH])≤5.0. If [PI] / ([PB]+[PH]) is 0.5 or more, heat resistance can be improved. [PI] / ([PB]+[PH]) is more preferably 1 or more. On the other hand, if [PI] / ([PB]+[PH]) is 5 or less, sensitivity can be improved. [PI] / ([PB]+[PH]) is more preferably 4 or less.

[0087] The relationship between [PB] and [PH] is preferably [PB]>[PH]. By making [PB]>[PH], the development adhesion can be improved. The relationship between [PI], [PB] and [PH] is preferably [PI]>[PB]>[PH]. By making [PI]>[PB]>[PH], the heat resistance of the cured product obtained by low temperature curing at about 200 to 270°C can be improved.

[0088] The mass ratio of [PB] to [PH] is preferably in the range of 1.01≤[PB] / [PH]≤55.00. When the mass ratio of [PB] / [PH] is 1.01 or more, the development adhesion can be improved. The mass ratio of [PB] / [PH] is more preferably 1.50 or more, and further preferably 2.00 or more. On the other hand, when the mass ratio of [PB] / [PH] is 55.00 or less, the sensitivity can be improved. The mass ratio of [PB] / [PH] is more preferably 30.00 or less, and further preferably 10.00 or less.

[0089] The positive photosensitive resin composition of the present invention contains (D) a quinonediazide compound.

[0090] By containing the (D) quinonediazide compound, an acid is generated in the light-irradiated portion, so that the solubility of the light-irradiated portion in the alkaline aqueous solution is increased, and a positive relief pattern in which the light-irradiated portion is dissolved can be obtained.

[0091] As the (D) quinonediazide compound, there can be mentioned compounds formed by ester bonding of quinonediazidesulfonic acid and polyhydroxy compounds, compounds formed by sulfonamide bonding of quinonediazidesulfonic acid and polyamino compounds, compounds formed by ester bonding and / or sulfonamide bonding of quinonediazidesulfonic acid and polyhydroxypolyamino compounds, etc. When the hydroxyl groups or amino groups of these polyhydroxy compounds and polyamino compounds in the (D) quinonediazide compound are taken as 100 mol%, it is preferred that 50 mol% or more are esterified or sulfonamidated with quinonediazidesulfonic acid. In addition, the positive photosensitive resin composition may contain two or more (D) quinonediazide compounds.

[0092] (D) The quinonediazide compound may appropriately contain a naphthoquinonediazidesulfonate compound. The naphthoquinonediazidesulfonate compound may be synthesized by an esterification reaction between a compound having a phenolic hydroxyl group and a quinonediazidesulfonic acid compound, and may be synthesized by a known method. By using these naphthoquinonediazidesulfonate compounds, the resolution, sensitivity, and residual film rate are further improved.

[0093] Examples of the compound having a phenolic hydroxyl group used herein include Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, MethyleneTris-FR-CR, BisRS-26X, DML-MBPC, DML-MBOC, DML-OCHP, DML-P CHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, Dimethylol-BisOC-P, DML-PFP, DML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BI Preferred examples include compounds obtained by introducing naphthoquinonediazide-4-sulfonic acid or naphthoquinonediazide-5-sulfonic acid through an ester bond into compounds such as OC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (trade names, manufactured by Asahi Organic Materials Industries, Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, and BisP-AP (trade names, manufactured by Honshu Chemical Industry Co., Ltd.), but compounds other than these may also be used.

[0094] The naphthoquinone diazide-4-sulfonate compound has absorption in the i-line region of a mercury lamp and is suitable for i-line exposure, while the naphthoquinone diazide-5-sulfonate compound has absorption extending to the g-line region of a mercury lamp and is suitable for g-line exposure. The photosensitive resin composition of the present invention may contain any of the naphthoquinone diazide-4-sulfonate compound and the naphthoquinone diazide-5-sulfonate compound, may contain a naphthoquinone diazide-sulfonate compound using both a naphthoquinone diazide-4-sulfonyl group and a naphthoquinone diazide-5-sulfonyl group in the same molecule, or may contain a mixture of a naphthoquinone diazide-4-sulfonate compound and a naphthoquinone diazide-5-sulfonate compound.

[0095] The content of the quinonediazide compound (D) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, relative to 100 parts by mass of the polyimide resin (A), from the viewpoint of improving sensitivity during exposure. In addition, from the viewpoint of reducing outgassing from the cured product, it is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, relative to 100 parts by mass of the polyimide resin (A).

[0096] The positive photosensitive resin composition of the present invention contains (E) a solvent.

[0097] By containing the (E) solvent, the composition can be in a varnish state, and coating properties can be improved.

[0098] The aforementioned (E) solvent may contain N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and other polar aprotic solvents, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tetrahydrofuran, dioxane and other ethers, acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, diacetone, etc., alone or in combination. Ketones such as alcohols, esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, methyl acetoacetate, ethyl acetoacetate and other esters, aromatic hydrocarbons such as toluene and xylene, and the like solvents.

[0099] From the viewpoint of improving coating properties, the solvent (E) preferably contains a polar aprotic solvent. As the aforementioned polar aprotic solvent, N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc. are preferred.

[0100] The content of the solvent (E) is preferably such that the solid content concentration of the positive photosensitive resin composition is 3 to 30% by mass. If the solid content concentration is less than 3% by mass, the coating property deteriorates, and it is more preferably 5% by mass or more. In addition, if the content of the solvent (E) is greater than 30% by mass, the storage stability of the positive photosensitive resin composition deteriorates, and it is more preferably 20% by mass or less.

[0101] Here, the solid content concentration refers to the concentration of components other than the (E) solvent in the positive photosensitive resin composition.

[0102] In addition, relative to 100% by mass of the aforementioned (E) solvent, the content of the aforementioned polar aprotic solvent is preferably 1 to 30% by mass. If it is 1% by mass or more, the solubility of the (A) component, the (B) component and the (C) component can be improved, and the linearity of the pattern after development can be improved. Relative to 100% by mass of the aforementioned (E) solvent, the content of the aforementioned polar aprotic solvent is more preferably 3% by mass or more. In addition, relative to 100% by mass of the aforementioned (E) solvent, when the content of the aforementioned polar aprotic solvent is 30% by mass or less, the solvent drying property during pre-baking is improved, and the development adhesion is improved. Relative to 100% by mass of the aforementioned (E) solvent, the content of the aforementioned polar aprotic solvent is more preferably 15% by mass or less, and further preferably 10% by mass or less.

[0103] The positive photosensitive resin composition of the present invention may contain a known compound such as a thermal crosslinking agent.

[0104] Examples of the thermal crosslinking agent include DML-PC, DML-PEP, DMOM-PC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP, HMOM-TPPA (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), "NIKALAC" (registered trademark) MX-270, "NIKALAC" (registered trademark) MW-100LM, (these are trade names, manufactured by Sanwa Chemical Co., Ltd.), and thermal crosslinking agents having a hydroxymethyl group and / or an alkoxymethyl group, "Denacol" EX-850L, "Denacol" EX-201-IM (these are trade names, manufactured by Nagase Chemtex Co., Ltd.), VG3101L (trade name, manufactured by Printex Co., Ltd.), "TEPIC" (registered trademark)-S, "TEPIC"-L, "TEPIC"-VL, "TEPIC"-FL, "TEPIC"-UC (these are trade names, manufactured by Nissan Chemical Industries, Ltd.), thermal crosslinking agents having an epoxy group such as OXT-121, OXT-221, OX-SQ-H, OXT-191, PNOX-1009, RSOX (these are trade names, manufactured by Toagosei Co., Ltd.), thermal crosslinking agents having an oxetane group such as 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide) Bismaleimide thermal crosslinking agents such as 1,5-bis(maleimide)butane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, aromatic polyisocyanates such as 4,4'-methylenebis(phenylene isocyanate) (MDI) and toluene diisocyanate (TDI); aliphatic polyisocyanates such as hexamethylene diisocyanate (HDI), trimethylene diisocyanate, 1,4-tetramethylene diisocyanate, pentamethylene diisocyanate and lysine diisocyanate; alicyclic polyisocyanate thermal crosslinking agents such as isophorone diisocyanate (IPDI) and 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI).

[0105] From the viewpoint of improving the chemical resistance of the cured product, the content of the thermal crosslinking agent is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more relative to 100 parts by mass of the component (A). In addition, from the viewpoint of being able to reduce outgassing from the cured product and further improve the reliability of the organic EL display device, the content of the thermal crosslinking agent is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and further preferably 20 parts by mass or less relative to 100 parts by mass of the component (A).

[0106] The positive photosensitive resin composition of the present invention may contain (F) a thermal acid generator. The so-called thermal acid generator is a compound that generates an acid by heating, and the thermal decomposition starting temperature of the thermal acid generator is preferably 120°C or more, more preferably 130°C or more, and further preferably 140°C or more. By setting the thermal decomposition temperature to 120°C or more, it is possible to prevent the generation of acid in the process of drying the applied positive photosensitive resin film by applying heat during pattern processing (sometimes also described as a pre-baking process). In addition, the thermal decomposition starting temperature of the (F) thermal acid generator is preferably 250°C or less, more preferably 240°C or less, and further preferably 230°C or less. By setting the thermal decomposition temperature to 250°C or less, sufficient acid can be generated in the heating process. In the present invention, by generating an acid in the heating process, the cross-linking reaction of the thermal cross-linking agent can be promoted, and as a result, the unreacted cross-linking groups remaining in the cured product can be greatly reduced. If unreacted crosslinking groups remain in the cured product, gas components will be generated during the reliability test, thereby causing undesirable phenomena such as reduced brightness and pixel shrinkage of the organic EL display device. However, the reliability of the organic EL display device can be greatly improved by utilizing the crosslinking promotion effect based on the acid generated by the thermal acid generator.

[0107] The (F) thermal acid generator in the positive photosensitive resin composition of the present invention only needs to have a function of generating an acid by heating, and compounds having a function of generating an acid by light such as ultraviolet rays in addition to heat are also included in the definition of the thermal acid generator. However, the (D) quinonediazide compound is defined as a compound not included in the (F) thermal acid generator even if it generates an acid by heating.

[0108] The acid generated by the (F) thermal acid generator is preferably a strong acid, for example, an arylsulfonic acid such as p-toluenesulfonic acid and benzenesulfonic acid, an alkylsulfonic acid such as methanesulfonic acid, ethanesulfonic acid and butanesulfonic acid, or camphorsulfonic acid.

[0109] (F) The thermal acid generator includes sulfonium salts, sulfonic acid esters, and the like. Two or more of these may be contained. Among the sulfonium salts, from the viewpoint of generating heat by heating, it is preferred to contain a compound selected from the group consisting of monoarylsulfonium salts and trialkylsulfonium salts.

[0110] (F) Among the thermal acid generators, it is preferred that a thermal acid generator having a sulfonic acid ester structure is contained because the reliability improvement effect of the organic EL display device is high. For example, methyl methanesulfonate, ethyl methanesulfonate, propyl methanesulfonate, butyl methanesulfonate, phenyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, propyl ethanesulfonate, butyl ethanesulfonate, phenyl ethanesulfonate, methyl propanesulfonate, ethyl propanesulfonate, propyl propanesulfonate, butyl propanesulfonate, phenyl propanesulfonate, methyl butanesulfonate, ethyl butanesulfonate, propyl butanesulfonate, butyl butanesulfonate, phenyl butanesulfonate, methyl octanesulfonate, ethyl octanesulfonate, propyl octanesulfonate, butyl octanesulfonate, phenyl octanesulfonate, methyl p-toluenesulfonate, ethyl p-toluenesulfonate, propyl p-toluenesulfonate, butyl p-toluenesulfonate, phenyl p-toluenesulfonate, methoxyphenyl methanesulfonate, methoxyethyl methanesulfonate, methoxyethyl p-toluenesulfonate, "Irgacure" (registered trademark) PAG103, PAG121 (trade name, BASF Japan (trade name), PA-411, PA-480 (trade name, Heraeus (KK)), etc., and other examples of thermal acid generators having a sulfonate structure include PAI-01, PAI-101, PAI-106, PAI-1001, PAI-1002, PAI-1003, PAI-1004 (trade name, Midori Kagaku (KK)), SP-082, SP-601, SP-606, SP-607, SP-612 (trade name, ADEKA (KK)), NIT, MIN, ILP-110, ILP-110N, ILP-118, ILP-113, PA-223, PA-298 (trade name, Heraeus (KK)), NAI-105, NAI-106, NAI-109 (trade name, Midori Kagaku Co., Ltd.), etc.

[0111] In addition, the (F) thermal acid generator particularly preferably includes a compound represented by formula (2). By making the (F) thermal acid generator include a compound represented by formula (2), the volatility of the (F) thermal acid generator during curing (heat treatment) is reduced, and the (F) thermal acid generator can efficiently generate acid during curing, and the cross-linking promotion effect becomes greater, thereby improving the reliability of the organic EL display device. In addition, by making the (F) thermal acid generator include a compound represented by formula (2), the solubility in the alkaline developer is easily improved compared to the case where the compound represented by formula (2) is not included, thereby improving the exposure sensitivity.

[0112] [Chemical formula 4]

[0113]

[0114] (In formula (2), R 15It is a divalent to tetravalent group having 1 to 10 carbon atoms. 16 Each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an ethynyl group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms. a represents an integer of 2 to 4.

[0115] From the viewpoint of not reducing the exposure sensitivity, in formula (2), R 15 is a divalent to tetravalent group having 1 to 6 carbon atoms which may have a substituent, R 16 Each is independently a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms which may have a substituent.

[0116] As examples of the compounds described in the above formula (2), compounds obtained by sulfonating the alcoholic hydroxyl group or phenolic hydroxyl group of a compound having multiple alcoholic hydroxyl groups (sometimes described as a polyol compound) or a compound having multiple phenolic hydroxyl groups (sometimes described as a polyphenol compound) with methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, octanesulfonic acid, p-toluenesulfonic acid, benzenesulfonic acid, etc. can be cited. Among the polyol compounds, specific examples of divalent alcohol compounds include methylene glycol, ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, etc. Among the polyol compounds, specific examples of trivalent or higher alcohol compounds include glycerol, butanetriol, pentanetriol, hexanetriol, heptanetriol, octanediol, nonanetriol, decanediol, pentaerythritol, etc. Specific examples of polyphenol compounds include dihydroxybenzene, trihydroxybenzene, tetrahydroxybenzene, etc.

[0117] The content of the compound represented by formula (2) is preferably 20% by mass or more in 100% by mass of the thermal acid generator (F), more preferably 50% by mass or more, further preferably 70% by mass or more, and particularly preferably 100% by mass, from the viewpoint of easily obtaining an effect of improving exposure sensitivity and an effect of improving the reliability of the organic EL display device.

[0118] From the viewpoint of further improving the reliability of the organic EL display device, when the total mass parts of the aforementioned (A) component and the aforementioned (B) component are 100 mass parts, the content of the (F) thermal acid generator is preferably 1 mass part or more, more preferably 2 mass parts or more, and even more preferably 3 mass parts or more. In addition, from the viewpoint of imparting high heat resistance to the cured product, when the total mass parts of the aforementioned (A) component and the aforementioned (B) component are 100 mass parts, the content of the (F) thermal acid generator is preferably 15 mass parts or less, more preferably 10 mass parts or less, and even more preferably 8 mass parts or less.

[0119] The positive photosensitive resin composition of the present invention may contain a colorant. The so-called colorant refers to a known organic pigment, inorganic pigment or dye. The colorant may preferably be an organic pigment and / or an inorganic pigment.

[0120] Examples of the organic pigment include diketopyrrolopyrrole pigments, azo pigments such as azo, disazo or polyazo, copper phthalocyanine, threne pigments, benzofuranone pigments or metal complex pigments.

[0121] Examples of the inorganic pigment include titanium oxide, zinc white, zinc sulfide, white lead, calcium carbonate, precipitated barium sulfate, white carbon, manganese violet, and cobalt violet.

[0122] Examples of the dye include azo dyes, anthraquinone dyes, condensed polycyclic aromatic carbonyl dyes, indigo dyes, carbonium dyes, phthalocyanine dyes, methine or polymethine dyes.

[0123] For the purpose of improving the contrast of the organic EL display device, the color of the colorant is preferably black that can block visible light in the entire wavelength range. It is preferred that the positive photosensitive resin composition contains at least one selected from organic pigments, inorganic pigments and dyes, and contains such a colorant that is black when the cured product is made. For this purpose, the above-mentioned black organic pigments and black inorganic pigments can be contained, and it is also possible to make it approximately black by mixing two or more organic pigments and dyes. In the case of approximately blackening, it can be obtained by mixing two or more organic pigments and dyes of the above-mentioned red, orange, yellow, purple, blue, green, etc. It should be noted that the positive photosensitive resin composition of the present invention itself does not necessarily need to be black, and a colorant that makes the cured product black by changing color during heat curing can also be used.

[0124] Among them, from the viewpoint of ensuring high heat resistance, it is preferred to contain an organic pigment and / or an inorganic pigment, and contain a colorant that is black when a cured product is made. In addition, from the viewpoint of ensuring high insulation, it is preferred to contain an organic pigment and / or a dye, and contain a colorant that is black when a cured product is made. That is, from the viewpoint of being able to simultaneously achieve high heat resistance and insulation, it is preferred to contain an organic pigment, and contain a colorant that is black when a cured product is made.

[0125] The content of the colorant is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more, based on the total amount of the positive photosensitive resin composition excluding the solvent, from the viewpoint of obtaining the colorability required for the cured product. In addition, from the viewpoint of obtaining good storage stability, it is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less, based on the total amount of the positive photosensitive resin composition excluding the solvent.

[0126] In the case where the positive photosensitive resin composition contains a pigment, it is preferred to contain a dispersant. By containing a dispersant, the colorant can be dispersed uniformly and stably in the positive photosensitive resin composition. The dispersant is not particularly limited, but is preferably a polymer dispersant. As the polymer dispersant, for example, polyester polymer dispersants, acrylic polymer dispersants, polyurethane polymer dispersants, polyallylamine polymer dispersants or carbodiimide dispersants can be cited. More specifically, the so-called polymer dispersant refers to a polymer compound whose main chain is formed by polyamino, polyether, polyester, polyurethane, polyacrylate, etc., and has polar groups such as amines, carboxylic acids, phosphoric acids, amine salts, carboxylates, and phosphates in the side chains or at the ends of the main chains. The polar group is adsorbed on the pigment and plays a role in stabilizing the dispersion of the pigment by utilizing the steric hindrance of the main chain polymer.

[0127] Dispersants can be classified into (polymer) dispersants having only an amine value, (polymer) dispersants having only an acid value, (polymer) dispersants having both an amine value and an acid value, or (polymer) dispersants having neither an amine value nor an acid value, but (polymer) dispersants having both an amine value and an acid value, (polymer) dispersants having only an amine value are preferred, and (polymer) dispersants having only an amine value are more preferred.

[0128] About the content of dispersant, from the viewpoint of obtaining good dispersion stability, relative to 100 parts by mass of pigment, preferably more than 1 part by mass, more preferably more than 3 parts by mass. In addition, from the viewpoint of maintaining the heat resistance of cured product, relative to 100 parts by mass of pigment, preferably less than 100 parts by mass, more preferably less than 50 parts by mass.

[0129] The positive photosensitive resin composition used in the present invention may contain a close fit improver. As a close fit improver, silane coupling agents such as vinyl trimethoxysilane, vinyl triethoxysilane, epoxy cyclohexyl ethyl trimethoxy silane, 3-glycidoxypropyl trimethoxy silane, 3-glycidoxypropyl triethoxy silane, p-phenyl trimethoxy silane, 3-aminopropyl trimethoxy silane, 3-aminopropyl triethoxy silane, N-phenyl-3-aminopropyl trimethoxy silane, zirconium oxide chelating agent, titanium chelating agent, aluminum chelating agent, and compounds obtained by reacting aromatic amine compounds with alkoxy-containing silicon compounds, etc., can be cited. Two or more of them can be contained. By containing these close fit improvers, the close fit with base substrates such as silicon wafers, ITO, SiO2, and silicon nitride can be improved in the case of developing the positive photosensitive resin film. In addition, the resistance to oxygen plasma and UV ozone treatment used for washing can be improved. The content of the adhesion improver is preferably 0.1 to 10% by mass based on the total amount of the positive photosensitive resin composition excluding the solvent.

[0130] The positive photosensitive resin composition used in the present invention may contain a surfactant as needed for the purpose of improving wettability with the substrate. The surfactant may be a commercially available compound, and specifically, as a silicone surfactant, there may be cited SH series, SD series, ST series of Dow Corning Toray Silicone Co., Ltd., BYK series of BYKChemie Japan KK, KP series of Shin-Etsu Silicone Co., Ltd., DISFOAM series of NOF Corporation, TSF series of Toshiba Silicones Co., Ltd., etc., and as a fluorine-based surfactant, there may be cited the "MEGAFACE (registered trademark)" series of Dainippon Ink Industries, Ltd., Fluorad series of Sumitomo 3M Ltd., "Surflon (registered trademark)" series of Asahi Glass Co., Ltd., "Asahi Guard (registered trademark)" series, EF series of Shin-Akita Chemical Co., Ltd., OMNOVA Solutions Inc., and examples of surfactants composed of acrylic acid and / or methacrylic acid polymers include, but are not limited to, the Polyflow series of Kyoeisha Chemical Co., Ltd. and the DISPARLON (registered trademark) series of Kusumoto Chemical Co., Ltd.

[0131] The content of the surfactant is preferably 0.001 to 1% by mass based on the total amount of the positive photosensitive resin composition excluding the solvent.

[0132] The positive photosensitive resin composition used in the present invention may contain a compound having a phenolic hydroxyl group as needed for the purpose of compensating for the alkali developability of the photosensitive resin composition. Examples of the compound having a phenolic hydroxyl group include Bis-Z, BisOC-Z, BisOPP-Z, BisP-CP, Bis26X-Z, BisOTBP-Z, BisOCHP-Z, BisOCR-CP, BisP-MZ, BisP-EZ, Bis26X-CP, BisP-PZ, BisP-IPZ, BisCRIPZ, BisOCP-IPZ, BisOIPP-CP, Bis26X-IPZ, BisOTBP-CP, TekP-4HBPA (Tetrakis P-DO-BPA), TrisPHAP, TrisP-PA, TrisP-PHBA, TrisP-SA, TrisOCR-PA, BisOFP-Z, BisRS-2P, BisPG-26X, BisRS-3P, BisOC-OCHP, BisPC-OCHP, Bis25X-OCHP, Bis26X-OCHP, B isOCHP-OC, Bis236T-OCHP, MethyleneTris-FR-CR, BisRS-26X, B isRS-OCHP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A (trade name, manufactured by Asahi Organic Materials Industries, Ltd.), 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,4-dihydroxyquinoline, 2,6-dihydroxyquinoline, 2,3-dihydroxyquinoxaline, anthracene-1,2,10-triol, anthracene-1,8,9-triol, 8-hydroxyquinoline, and the like. By containing these compounds having a phenolic hydroxyl group, the obtained positive photosensitive resin composition is almost insoluble in an alkaline developer before exposure, but easily dissolves in an alkaline developer after exposure, so that film loss due to development is small and development becomes easy in a short time. Therefore, the sensitivity is easily improved.

[0133] The content of the compound having a phenolic hydroxyl group is preferably 1% by mass or more and 20% by mass or less based on the total amount of the positive photosensitive resin composition excluding the solvent.

[0134] In addition, the positive photosensitive resin composition used in the present invention may contain inorganic particles. Preferred specific examples include silicon oxide, titanium oxide, barium titanate, aluminum oxide, talc, etc., but are not limited thereto. The primary particle size of these inorganic particles is preferably 100 nm or less, and more preferably 60 nm or less.

[0135] The content of the inorganic particles is preferably 5 to 90% by mass based on the total amount of the positive photosensitive resin composition excluding the solvent.

[0136] Next, the method for producing the positive photosensitive resin composition of the present invention is described. For example, the positive photosensitive resin composition can be obtained by dissolving the component (A), the component (B), the component (C), the quinonediazide compound (D), the solvent (E), and the adhesion improver, surfactant, colorant, inorganic particles, etc. used as needed.

[0137] As the dissolution method, stirring and heating can be mentioned. In the case of heating, the heating temperature is preferably set within a range that does not damage the performance of the positive photosensitive resin composition, usually room temperature to 80°C. In addition, the dissolution order of each component is not particularly limited. For example, a method of dissolving in sequence starting from compounds with low solubility can be mentioned. In addition, for components such as surfactants and some adhesion improvers that are prone to generate bubbles when stirred and dissolved, they can be added last after the other components are dissolved, thereby preventing poor dissolution of other components caused by the generation of bubbles.

[0138] The obtained positive photosensitive resin composition is preferably filtered using a filter to remove dirt. The filter pore size is, for example, 0.5 μm, 0.2 μm, 0.1 μm, 0.07 μm, 0.05 μm, 0.02 μm, etc., but is not limited thereto. The filter material includes polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., preferably polyethylene and nylon. When the positive photosensitive resin composition contains pigments and particles, it is preferred to use a filter with a pore size larger than their particle size.

[0139] The cured product of the present invention is a cured product obtained by curing a positive photosensitive resin composition. The cured product can be obtained by heat-treating the positive photosensitive resin composition. The heat treatment method can adopt a known method such as a method using a hot plate, an oven, infrared rays, etc. The preferred heat treatment conditions are described in the step of heat-treating the developed positive photosensitive resin film in the production method of the cured product (5) described later.

[0140] Next, a method for producing a cured film using the positive photosensitive resin composition of the present invention will be described in detail.

[0141] The method for manufacturing a solidified product comprises the following steps in sequence:

[0142] (1) a step of applying the positive photosensitive resin composition to a substrate to form a positive photosensitive resin film;

[0143] (2) a step of drying the positive photosensitive resin film (prebaking step);

[0144] (3) exposing the dried positive photosensitive resin film through a photomask;

[0145] (4) a step of developing the exposed positive photosensitive resin film; and

[0146] (5) A step of heating the developed positive photosensitive resin film.

[0147] In the step (1) of coating the positive photosensitive resin composition on a substrate to form a positive photosensitive resin film, the positive photosensitive resin composition of the present invention is coated by spin coating, slit coating, dip coating, spray coating, printing, etc. to obtain a positive photosensitive resin film of the positive photosensitive resin composition. Prior to coating, the substrate to be coated with the positive photosensitive resin composition may be pre-treated with the above-mentioned adhesion improving agent.

[0148] For example, the following method can be mentioned: using a solution obtained by dissolving 0.5 to 20% by mass of a close contact improver in a solvent such as isopropyl alcohol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, diethyl adipate, etc., to treat the substrate surface. As a method for treating the substrate surface, spin coating, slot die coating, rod coating, dip coating, spray coating, steam treatment, etc. can be mentioned.

[0149] In the step (2) of drying the positive photosensitive resin film, the coated positive photosensitive resin film is subjected to a reduced pressure drying treatment as needed, and then a heat treatment is performed at a temperature in the range of 50°C to 180°C for 1 minute to several hours using a hot plate, an oven, infrared rays, etc., thereby obtaining a positive photosensitive resin film.

[0150] Next, the step (3) of exposing the dried positive photosensitive resin film through a photomask is described. The positive photosensitive resin film is irradiated with chemical radiation through a photomask having a desired pattern. Chemical radiation used for exposure includes ultraviolet rays, visible rays, electron beams, X-rays, etc. In the present invention, i-rays (365nm), h-rays (405nm), and g-rays (436nm) of a mercury lamp are preferably used.

[0151] After irradiation with chemical rays, post-exposure baking can be performed. By performing post-exposure baking, effects such as improved resolution after development or increased allowable range of development conditions can be expected. Post-exposure baking can use an oven, a hot plate, infrared rays, a rapid annealing device or a laser annealing device, etc. The post-exposure baking temperature is preferably 50 to 180°C, and more preferably 60 to 150°C. The post-exposure baking time is preferably 10 seconds to several hours. If the post-exposure baking time is within the above range, the reaction proceeds well and the development time can sometimes be shortened.

[0152] In the step (4) of developing the exposed positive photosensitive resin film, the exposed positive photosensitive resin film is developed using a developer to remove the portion other than the exposed portion. The developer is preferably an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine.

[0153] In addition, according to circumstances, a solution obtained by combining polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, dimethylacrylamide, etc., alcohols such as methanol, ethanol, isopropanol, esters such as ethyl lactate, propylene glycol monomethyl ether acetate, ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, methyl isobutyl ketone, etc., or one or more of the above may be added to these alkaline aqueous solutions. The developing method may be spraying, immersion by spinning, dipping, ultrasonic waves, or the like.

[0154] Next, the pattern formed by development is preferably rinsed with distilled water. Here, alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to distilled water for rinsing.

[0155] Next, a step (5) of heat-treating the developed positive photosensitive resin film is implemented. The heat treatment can remove residual solvents and components with low heat resistance, thereby improving heat resistance and chemical resistance. The positive photosensitive resin composition of the present invention can form imide rings and oxazole rings by heat treatment, thereby improving heat resistance and chemical resistance. In addition, in the case of containing a thermal crosslinking agent, a thermal crosslinking reaction can be carried out by heat treatment, which can improve heat resistance and chemical resistance. From the viewpoint of improving the heat resistance of the cured product, the heating treatment temperature is preferably above 200°C, more preferably above 220°C, further preferably above 230°C, and particularly preferably above 240°C.

[0156] On the other hand, from the viewpoint of avoiding the influence of thermal degradation of the TFT element, it is preferably below 400°C, more preferably below 350°C, and further preferably below 270°C. Within this temperature range, the temperature can be raised in stages or continuously. Regarding the heating treatment time, from the viewpoint of improving the heat resistance of the cured product, it is preferably above 30 minutes, and more preferably above 45 minutes. In addition, from the viewpoint of productivity, it is preferably below 180 minutes, and more preferably below 120 minutes. For example, the following methods can be cited: a method of performing heat treatment at 150°C and 250°C for 60 minutes each; a method of performing heat treatment while linearly raising the temperature from room temperature to 250°C over 2 hours; and the like.

[0157] The cured product of the present invention is preferably a cured product formed from the positive photosensitive resin composition of the present invention. In another embodiment of the cured product of the present invention, when the compound represented by formula (3), the compound represented by formula (4) and the compound represented by formula (5) are analyzed by reaction pyrolysis GC / MS, and the detection peak intensity ratio thereof is 0.1 to 1 for the compound represented by formula (3) and 0.1 to 3 for the compound represented by formula (5), when the compound represented by formula (4) is set to 1.

[0158] [Chemical formula 5]

[0159]

[0160] (In formula (3), formula (4) and formula (5), R 17 ~R 23 Each independently represents a hydrogen atom or a monovalent organic group having 1 to 30 carbon atoms which may contain a hetero atom.

[0161] In formula (3), formula (4) and formula (5), examples of the monovalent organic group having 1 to 30 carbon atoms which may contain a hetero atom include an alkyl group, an alkenyl group, an alkynyl group and an aryl group.

[0162] The aforementioned alkyl group may be linear, branched, or cyclic. The number of carbon atoms of the linear and branched alkyl groups is usually 1 to 30, preferably 1 to 20, and more preferably 1 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. The number of carbon atoms of the cyclic alkyl group is usually 3 to 30, preferably 3 to 20, and more preferably 3 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, cyclohexyl, heptyl, octyl, nonyl, and decyl.

[0163] The alkenyl group may be straight-chain, branched or cyclic. The number of carbon atoms of the straight-chain and branched alkenyl groups is usually 2 to 30, preferably 2 to 20, and more preferably 2 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. The number of carbon atoms of the cyclic alkenyl group is usually 3 to 30, preferably 3 to 20, and more preferably 3 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. As the alkenyl group, for example, vinyl, propenyl, isopropenyl, butenyl, butenyl, pentenyl, hexenyl, nonenyl, decenyl and the like can be cited.

[0164] The alkynyl group may be straight-chain, branched or cyclic. The number of carbon atoms of the straight-chain and branched alkynyl groups is usually 2 to 30, preferably 2 to 20, and more preferably 2 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. The number of carbon atoms of the cyclic alkynyl group is usually 3 to 30, preferably 3 to 20, and more preferably 3 to 10 from the viewpoint of high heat resistance and maintaining high bending resistance of the cured product. Examples of the alkynyl group include ethynyl, propynyl, butynyl, pentynyl, and hexynyl.

[0165] The aforementioned aryl group is the remaining atomic group obtained by removing one hydrogen atom directly bonded to the carbon atom constituting the aromatic ring from an aromatic hydrocarbon, and includes aryl groups having a hydroxyl group, the aforementioned alkyl group, the aforementioned alkenyl group, and the aforementioned alkynyl group as functional groups. The number of carbon atoms of the aryl group is usually 6 to 30, preferably 6 to 20. As the aryl group, for example, phenyl, hydroxyphenyl, alkylphenyl, alkylhydroxyphenyl, etc. can be mentioned. From the viewpoint of achieving a balance between high heat resistance and bending resistance of the cured product, hydroxyphenyl and alkylhydroxyphenyl are preferred. As the alkylphenyl group, for example, methylphenyl, ethylphenyl, dimethylphenyl, propylphenyl, methylethylphenyl, propylphenyl, isopropylphenyl, butylphenyl, isobutylphenyl, tert-butylphenyl, pentylphenyl, hexylphenyl, cyclohexylphenyl, heptylphenyl, octylphenyl, nonylphenyl, decylphenyl, etc. can be mentioned. Examples of the alkylhydroxyphenyl group include methylhydroxyphenyl, ethylhydroxyphenyl, dimethylhydroxyphenyl, propylhydroxyphenyl, methylethylhydroxyphenyl, propylhydroxyphenyl, isopropylhydroxyphenyl, butylhydroxyphenyl, isobutylhydroxyphenyl, tert-butylhydroxyphenyl, pentylhydroxyphenyl, hexylhydroxyphenyl, cyclohexylhydroxyphenyl, heptylhydroxyphenyl, octylhydroxyphenyl, nonylhydroxyphenyl and decylhydroxyphenyl.

[0166] From the viewpoint of achieving a balance between high heat resistance and bending resistance of the cured product, R 2 , R 3 , R 4 At least one of them is an alkyl group, an alkenyl group, an alkynyl group, or an aryl group. It is more preferred that the alkyl group and the hydroxyphenyl group and / or the alkylhydroxyphenyl group are simultaneously contained.

[0167] When the cured product is analyzed by reaction pyrolysis GC / MS, the compound represented by formula (3), the compound represented by formula (4) and the compound represented by formula (5) are detected. In terms of the detection peak intensity ratio, when the compound represented by formula (4) is set to 1, the compound represented by formula (3) is 0.1 to 1, and the compound represented by formula (5) is 0.1 to 3. As a result, it is easy to obtain a cured product with high heat resistance and high bending resistance.

[0168] The compounds contained in the cured product of the present invention are described. The compound represented by formula (3) can be obtained, for example, as a structure or residue derived from (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene. The compound represented by formula (4) can be obtained, for example, as a structure or residue derived from (A) polyimide, a polyimide precursor and a copolymer thereof. The compound represented by formula (5) can be obtained, for example, as a structure or residue derived from (B) polybenzoxazole, a polybenzoxazole precursor and a copolymer thereof.

[0169] The cured product formed from the positive photosensitive resin composition of the present invention can be used in a display device including a first electrode formed on a substrate and a second electrode disposed opposite to the first electrode, specifically, a planarization layer of a liquid crystal display device, a planarization layer and / or a pixel segmentation layer of an organic EL display device, etc. The following description will be given by taking an organic EL display device as an example.

[0170] The organic EL display device of the present invention has the aforementioned solidified material. Specifically, it is preferably an organic EL display device having a driving circuit, a planarization layer, a first electrode, a pixel segmentation layer, a light-emitting layer and a second electrode on a substrate, and the planarization layer and / or the pixel segmentation layer contain the aforementioned solidified material. When taking an active matrix display device as an example, a thin film transistor (hereinafter referred to as TFT) and a wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as glass or a resin film, a planarization layer is provided thereon in a manner covering the concave and convex, and a display element is further provided on the planarization layer. The display element is connected to the wiring via a contact hole formed in the planarization layer. In particular, in recent years, the flexibility of organic EL display devices has become the mainstream, and an organic EL display device in which the aforementioned substrate having a driving circuit is formed by a resin film is preferred.

[0171] With regard to the organic EL display device of the present invention, it is preferred that at least a part of the portion having a cured product preferably has a bendable portion and / or a portion fixed in a bent state. By using a cured product obtained by curing the positive photosensitive resin composition or photosensitive resin sheet of the present invention, an organic EL display device with excellent bending resistance can be obtained. The radius of curvature of the above-mentioned bendable portion and / or the portion fixed in a bent state is preferably greater than 0.1 mm, preferably less than 5 mm. If the radius of curvature is greater than 0.1 mm, the bending resistance of the bent portion can be ensured, and if it is less than 5 mm, the appearance design such as narrow frame can be ensured.

[0172] The organic EL display device of the present invention can be bent at any appropriate part. For example, the organic EL display device can be bent in the center like a foldable display device, and can also be bent at the end from the perspective of maximizing the design and display screen. In addition, the organic EL display device can be bent along its long side direction or along its short side direction. Depending on the application, a specific part of the organic EL display device can be bent (for example, part or all of the four corners can be bent along the inclined direction).

[0173] Figure 1 A cross-sectional view of an example of an organic EL display device in which a planarization layer and a pixel division layer are formed is shown. On a substrate 6, bottom-gate or top-gate TFTs 1 are arranged in rows and columns, and a TFT insulating layer 3 is formed in a state of covering the TFTs 1. In addition, a wiring 2 connected to the TFTs 1 is provided on the TFT insulating layer 3. Furthermore, on the TFT insulating layer 3, a planarization layer 4 is provided in a state in which the wiring 2 is buried. In the planarization layer 4, a contact hole 7 is provided to reach the wiring 2. Then, through the contact hole 7, an ITO (transparent electrode) 5 is formed on the planarization layer 4 in a state of being connected to the wiring 2.

[0174] Here, ITO 5 becomes an electrode of a display element (e.g., an organic EL element). Then, a pixel division layer 8 is formed in a manner covering the periphery of ITO 5. The organic EL element may be a top emission type that releases light from the side opposite to the substrate 6, or a bottom emission type that extracts light from the substrate 6 side. As described above, an active matrix type organic EL display device in which a TFT 1 for driving the organic EL element is connected to each organic EL element can be obtained.

[0175] The TFT insulating layer 3, the planarization layer 4 and / or the pixel division layer 8 can be formed by the following steps as described above: a step of forming a positive photosensitive resin film formed from the positive photosensitive resin composition of the present invention; a step of exposing the positive photosensitive resin film; a step of developing the exposed positive photosensitive resin film and a step of heating the developed positive photosensitive resin film. An organic EL display device can be obtained by a manufacturing method having these steps.

[0176] In addition, the cured product formed by the positive photosensitive resin composition of the present invention can be used as an insulating film or protective film constituting an electronic component. Here, as electronic components, active components, resistors, capacitors, inductors, and other passive components having semiconductors such as transistors, diodes, integrated circuits (hereinafter referred to as ICs), and memories can be cited. In addition, electronic components using semiconductors are also referred to as semiconductor devices. As a specific example of a cured product in an electronic component, it can be suitably used for a passivation film of a semiconductor, a surface protective film of a semiconductor element, a TFT, etc., an interlayer insulating film in a multilayer wiring for high-density mounting of 2 to 10 layers, an insulating film of a touch panel display, a protective film, etc., but is not limited thereto, and various structures can be used.

[0177] In addition, the substrate surface on which the cured product is formed can be appropriately selected according to the application and process, and silicon, ceramics, metals, glass, epoxy resins, etc. can be cited, and multiple of them can also be arranged on the same surface. As an electronic device having a surface protective film, an interlayer insulating film, etc. configured with the cured product of the present invention, for example, an MRAM with low heat resistance can be cited. That is, the cured product of the present invention is suitable for the surface protective film use of MRAM.

[0178] In addition to MRAM, polymer ferroelectric RAM (PFRAM) and phase change RAM (PCRAM or Ovonics Unified Memory) which are expected to be the next generation memory are also likely to use new materials with lower heat resistance than previous memories. Therefore, the cured product of the present invention is also suitable for their surface protection film applications.

[0179] In addition, it can also be suitably used in fan-out wafer-level packaging (hereinafter referred to as fan-out WLP). Fan-out WLP is a semiconductor package in which an expansion portion is provided around a semiconductor chip using a sealing resin such as epoxy resin, and rewiring is performed from electrodes on the semiconductor chip to the expansion portion, and solder balls are also mounted on the expansion portion, thereby ensuring the necessary number of terminals.

[0180] In the fan-out WLP, wiring is provided so as to cross the boundary formed by the main surface of the semiconductor chip and the main surface of the sealing resin. That is, an interlayer insulating film is formed on a substrate composed of two or more materials, namely, a semiconductor chip with metal wiring applied thereto and a sealing resin, and wiring is formed on the interlayer insulating film.

[0181] In addition, in a semiconductor package of a type in which a semiconductor chip is embedded in a recess formed on a glass epoxy resin substrate, wiring is also provided in a manner that spans the boundary line between the main surface of the semiconductor chip and the main surface of the printed circuit board. In this manner, an interlayer insulating film is also formed on a substrate composed of two or more materials, and wiring is formed on the interlayer insulating film. The cured product formed by curing the positive photosensitive resin composition of the present invention has high adhesion to a semiconductor chip to which metal wiring is applied, and also has high adhesion to a sealing resin such as an epoxy resin, and therefore, can be suitably used as an interlayer insulating film provided on a substrate composed of two or more materials.

[0182] Example

[0183] Hereinafter, the present invention will be described with reference to Examples etc., but the present invention is not limited to these Examples. In addition, the evaluation of the positive photosensitive resin composition in the Examples was performed by the following method.

[0184] (1) Sensitivity evaluation

[0185] The positive photosensitive resin composition obtained by each of the examples and comparative examples described below was applied to an 8-inch silicon wafer by spin coating using a coating and developing device ACT-8 (manufactured by Tokyo Electron Co., Ltd.), and baked at 120° C. for 3 minutes using a hot plate to prepare a pre-baked film with a film thickness of 3.0 μm. It should be noted that the film thickness was measured using Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd. under the condition of a refractive index of 1.63.

[0186] Then, an exposure machine i-line stepper NSR-2005i9C (manufactured by Nikon Corporation) was used to expose the film at 50 to 300 mJ / cm through a mask having a pattern of contact holes of 10 μm. 2 The exposure dose is 10mJ / cm 2 After exposure, the film was developed using the ACT-8 developing device described above, using a 2.38 mass % tetramethylammonium aqueous solution (hereinafter referred to as TMAH, manufactured by Tama Chemical Industry Co., Ltd.) for a time period in which the film loss during development was 0.5 μm, and then rinsed with distilled water and spun dry to obtain a pattern.

[0187] The pattern of the developed film was observed at a magnification of 20 times using an FDP microscope MX61 (manufactured by Olympus Corporation) to determine the minimum exposure required for the opening diameter of the contact hole to be 10 μm. This was taken as the exposure sensitivity, and 200 mJ / cm 2 The smaller the value of the sensitivity, the higher the sensitivity, which is more preferred.

[0188] (2) Bending resistance evaluation

[0189] The positive photosensitive resin composition obtained by each of the examples and comparative examples described later was applied to a polyimide film substrate at an arbitrary rotation speed by spin coating to obtain a positive photosensitive resin film. As a drying process, it was pre-baked on a hot plate at 120°C for 2 minutes to obtain a positive photosensitive resin film. Next, an automatic developing device (AD-2000 manufactured by TakizawaSangyo Co., Ltd.) was used to perform spray development for 90 seconds using a 2.38% by mass tetramethylammonium hydroxide aqueous solution, followed by rinsing with pure water for 30 seconds. Under a nitrogen atmosphere, the developed substrate with the positive photosensitive resin film was cured (heat treated) for 60 minutes in an oven at 250°C to obtain a cured product with a film thickness of 2.0 μm.

[0190] Next, 10 polyimide film substrates with cured products were cut out in a size of 50 mm in length and 10 mm in width. Next, the cut polyimide film was stored at 100 ° C for 500 hours in an air atmosphere. Then, the surface of the cured product was made to be outside, and the polyimide film substrate was bent 180 ° on a line of 25 mm in the longitudinal direction and kept for 30 seconds. After 30 seconds, the bent polyimide film substrate was opened, and an FPD inspection microscope (MX-61L; Olympus (Strain) was used to observe the bent portion on the line of 25 mm in the longitudinal direction on the surface of the cured product, and the appearance change of the surface of the cured product was evaluated. The bending test was implemented in the range of a curvature radius of 0.1 to 2.0 mm, and the minimum curvature radius (mm) without peeling of the cured product from the polyimide film substrate, cracks on the surface of the cured product, and other appearance changes was recorded. The smaller the value of the minimum curvature radius (mm), the higher the bending resistance, and the more preferred.

[0191] (3) Reliability test of organic EL display device

[0192] <Production of Organic EL Display Device>

[0193] Figure 2A schematic diagram of the substrate used is shown in the figure. First, on a 38×46 mm alkali-free glass substrate 11, an ITO transparent conductive film of 100 nm is formed on the entire surface of the substrate by sputtering, and then etched into a first electrode 12. In addition, at the same time, in order to take out the second electrode, an auxiliary electrode 13 is also formed at the same time. The obtained substrate is ultrasonically cleaned for 10 minutes using "Semico Clean 56" (trade name, manufactured by Furuuchi Chemical Co., Ltd.), and then washed with ultrapure water. Next, a positive photosensitive resin composition (varnish) according to each of the embodiments and comparative examples described later is applied to the entire surface of the substrate by spin coating, and pre-baked on a hot plate at 120°C for 2 minutes. For the film, a parallel photomask aligner (hereinafter referred to as PLA) (PLA-501F manufactured by Canon Corporation) was used, and an ultra-high pressure mercury lamp was used as a light source (mixed line of g-line, h-line, and i-line). After UV exposure through a photomask, it was developed using a 2.38% TMAH aqueous solution, and only the exposed part was dissolved, and then rinsed with pure water. For the resulting patterned substrate, an inert oven (CLH-21CD-S manufactured by Koyo Thermo Systems Co., Ltd.) was used to cure it in an oven at 250°C for 60 minutes under a nitrogen atmosphere. As described above, openings with a width of 50 μm and a length of 260 μm are arranged at a pitch of 155 μm in the width direction and a pitch of 465 μm in the length direction, and the pixel segmentation layer 14 of the shape in which each opening exposes the first electrode is formed only in the effective area of ​​the substrate. As described above, a pixel division layer having an aperture ratio of 18% is provided in a quadrilateral substrate effective area having a side of 16 mm, and the thickness of the pixel division layer is about 2.0 μm.

[0194] Next, as a pre-treatment, nitrogen plasma treatment was performed, and then the organic EL layer 15 was formed by vacuum deposition. It should be noted that the vacuum degree during the deposition was 1×10 -3 Pa or less, and during the evaporation, the substrate is rotated relative to the evaporation source. First, 10 nm of compound (HT-1) is evaporated as a hole injection layer, and 50 nm of compound (HT-2) is evaporated as a hole transport layer. Next, on the light-emitting layer, compound (GH-1) as a main material and compound (GD-1) as a dopant material are evaporated to a thickness of 40 nm in such a way that the doping concentration becomes 10%. Next, as an electron transport material, compound (ET-1) and compound (LiQ) are stacked in a volume ratio of 1:1 to a thickness of 40 nm. The structure of the compounds used in the organic EL layer is shown below.

[0195] [Chemical formula 6]

[0196]

[0197] Next, after evaporating 2 nm of the compound (LiQ), Mg and Ag were evaporated to 60 nm at a volume ratio of 1:10 to form the second electrode 16. Finally, in a low-humidity nitrogen atmosphere, the cap-shaped glass plate was bonded using an epoxy resin adhesive to seal it, and four light-emitting devices (which were quadrilaterals with each side of 5 mm) were made on one substrate. It should be noted that the film thickness here is the display value of the quartz oscillation film thickness monitor.

[0198] <Reliability Evaluation>

[0199] In an air atmosphere, the organic EL display device is stored at 100°C, and the organic EL display device is taken out every 100 hours, and it is driven by direct current at 10 mA / cm2 to emit light, and the luminous area in the luminous pixel is measured. When the initial luminous area before the reliability test is set to 100, the shortest time for the luminous area after the UV irradiation treatment test to be less than 50 is taken as the reliability of the organic EL display device (unit: hours), and the reliability is considered to be qualified when it is more than 500 hours. The longer the shortest time for the luminous area after the UV irradiation treatment test to be less than 50, the better the reliability, and therefore the more preferred.

[0200] (4) Heat resistance evaluation

[0201] Using a coating and developing device ACT-8 (manufactured by Tokyo Electron Co., Ltd.), the positive photosensitive resin composition obtained by the following examples and comparative examples was applied to an 8-inch silicon wafer by spin coating, and baked at 120°C using a hot plate for 3 minutes to produce a pre-baked film with a film thickness of 3.0 μm. Then, using the aforementioned ACT-8 developing device, a 2.38% by mass tetramethylammonium aqueous solution (hereinafter referred to as TMAH, manufactured by Tama Chemical Industry Co., Ltd.) was used to develop the film for a time at which the film loss during development was 0.5 μm, and then rinsed with distilled water and dried. Then, using an inert oven (CLH-21CD-S manufactured by Koyo ThermoSystems Co., Ltd.), the film was cured in an oven at 250°C for 60 minutes under a nitrogen atmosphere. The resulting cured product was peeled off using hydrofluoric acid to obtain a film. 10 mg of the obtained single film was loaded into an Al fixture unit to prepare a TGA measurement sample, and thermogravimetric measurement was performed using TGA-50 (manufactured by Shimadzu Corporation) in a nitrogen atmosphere while heating at 10°C per minute. Regarding the temperature at which the weight was reduced by 5% compared to the weight at 200°C, 320°C or above was considered acceptable. The higher the temperature at which the weight was reduced by 5% compared to the weight at 200°C, the higher the heat resistance, which is more preferred.

[0202] (5) Evaluation of Development Adhesion

[0203] Using a coating and developing device ACT-8 (manufactured by Tokyo Electron Co., Ltd.), the positive photosensitive resin composition obtained by the following examples and comparative examples was applied to an 8-inch silicon wafer by spin coating, and baked at 120°C using a hot plate for 3 minutes to produce a pre-baked film with a film thickness of 3.0 μm. It should be noted that the film thickness was measured using Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd. under the condition of a refractive index of 1.63. Then, using an exposure machine i-line stepper NSR-2005i9C (manufactured by Nikon Corporation), exposure was performed with an exposure amount of the exposure sensitivity obtained in (1) through a mask having a pattern of a large number of closed portions with a diameter of 3 to 100 μm. After exposure, the ACT-8 developing device is used, and a 2.38 mass % tetramethylammonium aqueous solution (hereinafter referred to as TMAH, manufactured by Tama Chemical Industry Co., Ltd.) is used for development for a time at which the film loss during development is 0.5 μm. The film is then rinsed with distilled water and spun dry to obtain a pattern.

[0204] The pattern of the obtained developed film was observed at a magnification of 20 times using an FDP microscope MX61 (manufactured by Olympus Corporation), and 100 locations were observed per unit size. The minimum closed pattern in which 90 or more patterns were not peeled off and remained was confirmed. If the pattern of 10 μm or less was not peeled off and remained, it was considered to be qualified. The smaller the minimum closed pattern in which 90 or more patterns were not peeled off and remained, the better the development adhesion, and therefore the more preferred it is.

[0205] (6) Evaluation of pattern linearity after development

[0206] The pattern of the developed film obtained in (5) was observed at a magnification of 20 times using an FDP microscope MX61 (manufactured by Olympus Corporation), and the 50 μm closed pattern was observed at 100 locations. If there were no shape abnormalities in more than 90 patterns, it was considered good (A); if there were no shape abnormalities in more than 80 patterns, it was considered slightly good (B); if there were less than 80 patterns without shape abnormalities, it was considered poor (C).

[0207] <Composition analysis based on reaction pyrolysis GC / MS>

[0208] After adding 3 μL of the reaction reagent (tetramethylammonium hydroxide) to 61 μg of the cured product obtained in (4), thermal cracking was carried out at a heating temperature of 400°C using a Multi Shot Pyrolyzer PY-3030D (manufactured by Frontier Lab), and analysis was carried out using a gas chromatograph-mass spectrometer JMS-Q1000GC (K9) (manufactured by JEOL), a stainless steel capillary column (0.25 mm inner diameter × 30 m, stationary phase; 5% phenyl polydimethylsiloxane) was used as the GC column, the GC temperature was increased from 40°C (maintained for 3 minutes) to 320°C at a rate of 20°C / min, the injection port temperature was 300°C, the column flow rate was 1.5 mL / min, the ionization method was the EI (electron ionization) method, the mass number range was set to m / z 20 to 800, and the scanning speed was set to 0.5 sec / scan.

[0209] The compounds used in Examples and Comparative Examples are shown below.

[0210] Synthesis Example 1 Synthesis of a hydroxyl-containing diamine compound

[0211] 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter referred to as BAHF) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide, and the mixture was cooled to -15°C. A solution obtained by dissolving 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride in 100 mL of acetone was added dropwise thereto. After completion of the dropwise addition, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was separated by filtration and vacuum dried at 50°C.

[0212] 30 g of the solid was placed in a 300 mL stainless steel autoclave, dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon was added. Hydrogen was introduced into the mixture using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, it was confirmed that the balloon was no longer deflated, and the reaction was terminated. After the reaction was completed, the palladium compound as a catalyst was removed by filtration, and concentrated using a rotary evaporator to obtain a hydroxyl-containing diamine compound represented by the following formula.

[0213] [Chemical formula 7]

[0214]

[0215] Synthesis Example 2 Synthesis of polyimide precursor (P1)

[0216] Under a dry nitrogen stream, 62.0 g (0.20 mole) of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (hereinafter referred to as ODPA) was dissolved in 500 g of N-methyl-2-pyrrolidone (hereinafter referred to as NMP). 96.7 g (0.16 mole) of the hydroxyl-containing diamine compound obtained in Synthesis Example 1 was added together with 100 g of NMP, and the reaction was carried out at 20°C for 1 hour, and then at 50°C for 2 hours. Next, 8.7 g (0.08 mole) of 3-aminophenol as a capping agent was added together with 50 g of NMP, and the reaction was carried out at 50°C for 2 hours. Then, a solution obtained by diluting 47.7 g (0.40 mole) of N,N-dimethylformamide dimethyl acetal with 100 g of NMP was added dropwise over 10 minutes. After the addition, the mixture was stirred at 50°C for 3 hours. After the stirring was completed, the solution was cooled to room temperature and then poured into 5 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed with water three times, and then dried in a vacuum dryer at 80° C. for 24 hours to obtain the target polyimide precursor (P1).

[0217] Synthesis Example 3 Synthesis of polyimide (P2)

[0218] Under a dry nitrogen stream, 58.6 g (0.16 mole) of BAHF and 8.7 g (0.08 mole) of 3-aminophenol as a capping agent were dissolved in 300 g of N-methyl-2-pyrrolidone (NMP). 62.0 g (0.20 mole) of ODPA was added together with 100 g of NMP, stirred at 20 ° C for 1 hour, and then stirred at 50 ° C for 4 hours. Then, 15 g of xylene was added, and water and xylene were azeotroped together while stirring at 150 ° C for 5 hours. After stirring, the solution was put into 5 L of water and a white precipitate was collected. The precipitate was collected by filtration, washed with water 3 times, and dried in a vacuum dryer at 80 ° C for 24 hours to obtain the target polyimide (P2).

[0219] Synthesis Example 4 Synthesis of polybenzoxazole precursor (P3)

[0220] Under a dry nitrogen stream, 0.16 mol of a mixture of dicarboxylic acid derivatives obtained by reacting 41.3 g (0.16 mol) of diphenyl ether-4,4'-dicarboxylic acid and 43.2 g (0.32 mol) of 1-hydroxy-1,2,3-benzotriazole and 73.3 g (0.20 mol) of BAHF were dissolved in 570 g of NMP, and then reacted at 75°C for 12 hours. Next, 13.1 g (0.08 mol) of 5-norbornene-2,3-dicarboxylic anhydride dissolved in 70 g of NMP was added, and the reaction was further stirred for 12 hours to terminate the reaction. After filtering the reaction mixture, the reaction mixture was put into a solution of water / methanol = 3 / 1 (volume ratio) to obtain a white precipitate. The precipitate was collected by filtration, washed with water 3 times, and dried in a vacuum dryer at 80°C for 24 hours to obtain the target polybenzoxazole (PBO) precursor (P3). P3 has the structural unit represented by the above-mentioned formula (1).

[0221] Synthesis Example 5 Synthesis of polyhydroxystyrene (P4)

[0222] To the mixed solution obtained by adding 2.56 g (0.04 mole) of sec-butyl lithium as an initiator to 2400 g of tetrahydrofuran, 105.75 g (0.6 mole) of p-tert-butoxystyrene was added, and after polymerization was carried out while stirring for 3 hours, 12.82 g (0.4 mole) of methanol was added to stop the polymerization reaction. Next, in order to purify the polymer, the reaction mixture was injected into 3 L of methanol, and the precipitated polymer was dried. The obtained polymer was dissolved in 1.6 L of acetone, 2 g of concentrated hydrochloric acid was added at 60°C, and stirred for 7 hours, and p-tert-butoxystyrene was deprotected to convert it into hydroxystyrene. After the reaction was completed, the solution was injected into water to precipitate the polymer. After washing the obtained precipitate with water 3 times, it was dried in a vacuum dryer at 50°C for 24 hours to obtain the target polyhydroxystyrene (P4).

[0223] Synthesis Example 6 Synthesis of acrylic resin (P5)

[0224] A methyl methacrylate / methacrylic acid / styrene copolymer (mass ratio of 30 / 40 / 30) was synthesized by a known method (Japanese Patent No. 3120476; Example 1). 40 parts by mass of glycidyl methacrylate was added to 100 parts by mass of the copolymer, and the mixture was reprecipitated with purified water, filtered, and dried to obtain an acrylic resin (P5) which is a polymer containing a free radical polymerizable monomer.

[0225] Synthesis Example 7 Synthesis of Quinone Diazide Compounds

[0226] Under a dry nitrogen stream, 21.22 g (0.05 mole) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 36.27 g (0.135 mole) of naphthoquinone diazide-5-sulfonyl chloride were dissolved in 450 g of 1,4-dioxane and the mixture was brought to room temperature. 15.18 g of triethylamine mixed with 50 g of 1,4-dioxane was added dropwise thereto in such a manner that the temperature in the system did not rise above 35°C. After the addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered and the filtrate was put into water. The precipitate was then collected by filtration. The precipitate was dried using a vacuum dryer to obtain a quinonediazide compound 1 represented by the following formula.

[0227] [Chemical formula 8]

[0228]

[0229] <Thermal Crosslinking Agent Having Epoxy Group>

[0230] TEPIC-VL: "TEPIC" (registered trademark)-VL (epoxy thermal crosslinking agent containing an isocyanuric acid ring structure, a compound represented by the following chemical formula, manufactured by Nissan Chemical Industries, Ltd.)

[0231] [Chemical formula 9]

[0232]

[0233] <Thermal Acid Generator>

[0234] BTS: butyl p-toluenesulfonate (a thermal acid generator having a sulfonate structure but not satisfying formula (2), manufactured by FUJIFILM Wako Pure Chemical Corporation)

[0235] F1: 1,3-propanediol di-p-toluenesulfonate (a thermal acid generator having a sulfonate structure and satisfying formula (2), manufactured by FUJIFILM Wako Pure Chemical Corporation)

[0236] F2: 1,4-butanediol dimethanesulfonate (a thermal acid generator having a sulfonate structure and satisfying formula (2), manufactured by Tokyo Chemical Industry Co., Ltd.)

[0237] [Chemical formula 10]

[0238]

[0239] <Solvent>

[0240] PGME: Propylene glycol monomethyl ether

[0241] GBL: gamma-butyrolactone

[0242] Example 1

[0243] Under a yellow light, 100 g of (P1) obtained in Synthesis Example 2 as component (A), 65 g of (P3) obtained in Synthesis Example 4 as component (B), 25 g of (P4) obtained in Synthesis Example 5 as component (C), 20 g of quinonediazide compound 1 obtained in Synthesis Example 7 as quinonediazide compound (D), and 15 g of TEPIC-VL as a thermal crosslinking agent were weighed and dissolved in 1823 g of PGME and 203 g of GBL. The obtained solution was then filtered using a filter having a pore size of 1 μm to obtain a positive photosensitive resin composition A. The obtained positive photosensitive resin composition was used to perform the evaluations of (1) to (6) above.

[0244] Examples 2 to 19, Comparative Examples 1 to 7

[0245] Positive photosensitive resin compositions B to S and positive photosensitive resin compositions a to g were obtained in the same manner as in Example 1, with the types and amounts of the compounds being as shown in Tables 1 and 2. The evaluations (1) to (6) above were carried out using the obtained positive photosensitive resin compositions.

[0246] Tables 1 and 2 show the compositions and evaluation results of Examples and Comparative Examples.

[0247] [Table 1-1]

[0248]

[0249] [Table 1-2]

[0250]

[0251] [Table 2]

[0252]

[0253] Examples 1 to 19 all obtained good results in all aspects of sensitivity, bending resistance, reliability of the organic EL display device, heat resistance, development adhesion, and pattern linearity. In contrast, the result of Comparative Example 1, which did not use component (A), was poor in reliability and heat resistance. The results of Comparative Examples 2 and 7, which had a large amount of component (C), were poor in development adhesion. The result of Comparative Example 3, which had a large amount of component (B), was poor in heat resistance. The results of Comparative Examples 4 and 6, which had a small amount of component (B), were poor in bending resistance. The result of Comparative Example 5, which did not use component (C), was poor in sensitivity.

[0254] Embodiment 20

[0255] The thermal decomposition product of the cured product of the photosensitive resin composition O was analyzed by the method described in the above <Composition analysis based on reaction thermal decomposition GC / MS>. As a result of the analysis, the structure obtained in the cured product is shown below, and a peak (1015 to 1025 seconds) belonging to the structure represented by formula (3), a peak (1335 to 1345 seconds) belonging to the structure represented by formula (4), and a peak (1860 to 1870 seconds) belonging to the structure represented by formula (5) were obtained.

[0256] [Chemical formula 11]

[0257]

[0258] These results confirmed that, in the cured product of the photosensitive resin composition O, the compound represented by formula (3), the compound represented by formula (4) and the compound represented by formula (5) were detected in the cured product, and that, with respect to the detection peak intensity ratio, when the compound represented by formula (4) was set to 1, the compound represented by formula (3) was 0.5, and the compound represented by formula (5) was 1.

[0259] Description of Reference Numerals

[0260] 1: Substrate

[0261] 2: TFT

[0262] 3: TFT insulation layer

[0263] 4: Wiring

[0264] 5: Flattening layer

[0265] 6: Contact hole

[0266] 7: First electrode

[0267] 8: Pixel segmentation layer

[0268] 9: Organic EL layer

[0269] 10: Second electrode

[0270] 11: Glass substrate

[0271] 12: First electrode

[0272] 13: Auxiliary electrode

[0273] 14: Pixel segmentation layer

[0274] 15: Organic EL layer

[0275] 16: Second electrode

Claims

1. A positive photosensitive resin composition comprising: (A) one or more selected from the group consisting of polyimide, polyimide precursor and copolymers thereof; (B) at least one selected from the group consisting of polybenzoxazole, polybenzoxazole precursor, and copolymers thereof; (C) polyhydroxystyrene and / or a copolymer of polyhydroxystyrene and polystyrene; (D) quinonediazide compounds; and (E) a solvent, The content of the component (B) is 10 to 100 parts by mass based on 100 parts by mass of the component (A). The content of the component (C) is 1 to 90 parts by mass based on 100 parts by mass of the component (A).

2. The positive photosensitive resin composition according to claim 1, wherein When the content of the component (A) is [PI] (mass), the content of the component (B) is [PB] (mass), and the content of the component (C) is [PH] (mass), The mass ratio [PI] / ([PB]+[PH]) is in the range of 0.5≤[PI] / ([PB]+[PH])≤5.

0.

3. The positive photosensitive resin composition according to claim 2, wherein The relationship between [PB] and [PH] is [PB]>[PH].

4. The positive photosensitive resin composition according to claim 3, wherein The mass ratio of [PB] to [PH] is in the range of 1.01≤[PB] / [PH]≤55.

00.

5. The positive photosensitive resin composition according to claim 1, wherein The component (C) contains polyhydroxystyrene.

6. The positive photosensitive resin composition according to claim 1, wherein The (E) solvent includes a polar aprotic solvent.

7. The positive photosensitive resin composition according to claim 6, wherein The content of the polar aprotic solvent is 1 to 30% by mass relative to 100% by mass of the (E) solvent. 8 . The positive photosensitive resin composition according to claim 1 , wherein the solid content concentration of the positive photosensitive resin composition is 3 to 30% by mass.

9. The positive photosensitive resin composition according to claim 1, wherein The component (B) comprises a resin having a structural unit represented by formula (1) as a main chain, [Chemical formula 1] In formula (1), R 1 and R 2 Each independently represents a divalent to octavalent organic group having 2 to 30 carbon atoms; p represents an integer of 0 to 4; and q represents an integer of 1 to 4. 10 . The positive photosensitive resin composition according to claim 1 , further comprising (F) a thermal acid generator.

11. The positive photosensitive resin composition according to claim 10, wherein The (F) thermal acid generator contains a thermal acid generator having a sulfonate structure.

12. The positive photosensitive resin composition according to claim 10, wherein The (F) thermal acid generator contains a compound represented by formula (2), [Chemical formula 2] In formula (2), R 15 is a divalent to tetravalent group having 1 to 10 carbon atoms; R 16 Each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent or an aryl group having 6 to 20 carbon atoms which may have a substituent; examples of the substituent include a hydroxyl group, a halogen atom, a cyano group, a vinyl group, an ethynyl group, or a linear or cyclic alkyl group having 1 to 10 carbon atoms; and a represents an integer of 2 to 4.

13. A cured product obtained by curing the positive photosensitive resin composition according to claim 1.

14. A solidified product, wherein When the reaction pyrolysis GC / MS was used for analysis, the compound represented by formula (3), the compound represented by formula (4) and the compound represented by formula (5) were detected. When the compound represented by formula (4) was set to 1, the compound represented by formula (3) was 0.1 to 1, and the compound represented by formula (5) was 0.1 to 3. [Chemical formula 3] In formula (3), formula (4) and formula (5), R 17 ~R 23 Each independently represents a hydrogen atom or a monovalent organic group having 1 to 30 carbon atoms which may contain a hetero atom.

15. An organic EL display device comprising the cured product according to claim 13 or 14.

16. A method for producing a solidified product, the method comprising the following steps in sequence: (1) a step of applying the positive photosensitive resin composition according to any one of claims 1 to 12 to a substrate to form a positive photosensitive resin film; (2) a step of drying the positive photosensitive resin film; (3) exposing the dried positive photosensitive resin film through a photomask; (4) a step of developing the exposed positive photosensitive resin film; and (5) A step of heating the developed positive photosensitive resin film.