High-strength progressive bone fracture plate and preparation method
By designing a multi-filled pore structure skeleton and high-density segments in the bone plate, combined with the preparation of the mixture of polymer fiber materials and polyether ether ketone powder, the problem that the existing bone plate is easy to break under high load is solved, and the bone plate is improved. The strength and biomechanical properties promote fracture healing and reduce costs.
Patent Information
- Application Number
- CN202410813294.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Due to the large elastic modulus difference between the elastic modulus of metal materials and human cortical bone, existing bone plates lead to problems such as stress shielding. Moreover, carbon fiber materials are prone to breakage and delamination at high loads, and cannot effectively support fracture healing.
High-strength progressive bone plates are prepared by mixing polymer fiber materials or metal materials with polyether ether ketone powder. Through the multi-filled pore structural skeleton design, high-density reinforcement sections, medium-density support sections and low-density connecting sections are set up, combined with polymer Material filling and sintering processes improve the strength and biomechanical properties of the bone plate.
It achieves the stability and biomechanical compatibility of the bone plate under high load conditions, avoids breakage and delamination problems, promotes fracture healing, and reduces material use and production costs.
Smart Images

Figure CN118750133A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a bone fracture plate, in particular to a high-strength progressive bone fracture plate and a preparation method thereof. Background Art
[0003] Bone plates are commonly used devices for internal fixation of fractures. They provide fixed support for the fractured bones of the human body, reduce the stress on the fracture ends, and promote normal healing of fractures.
[0004] The existing manufacturing method of bone plates is usually to use pure metal materials. However, since the elastic modulus of metal materials is quite different from that of human cortical bone, stress shielding and other problems may occur during use. In order to solve this problem, more and more continuous carbon fiber or chopped carbon fiber materials are mixed with polyetheretherketone and processed by injection molding, high-temperature pressing and other methods. In this type of bone plates, since the carbon fiber filaments are evenly distributed in the polyetheretherketone matrix in the form of prepreg tapes, the interfacial bonding force between the two is low. When applied to parts of the human body with higher bearing capacity, the bone plates are prone to technical problems such as breakage and delamination. Summary of the invention
[0006] In view of the above technical problems, the present invention provides a high-strength progressive bone plate and a preparation method. In the high-strength progressive bone plate and the preparation method, the density of the middle position of the bone plate is higher, and the density of the two sides gradually decreases to form a progressive structure. The high-density structure at the center position provides high-strength support for the bone plate.
[0007] More importantly, this preparation method uses a mixture of polymer fiber materials or metal materials and polyetheretherketone powder. The two have a high bonding strength and can be easily applied to parts of the human body with higher bearing capacity. The bone plate is not prone to technical problems such as breakage and delamination.
[0008] To this end, the technical solution of the present invention is a high-strength progressive bone plate, which is provided with a multi-filled pore bone plate structural skeleton, the multi-filled pore bone plate structural skeleton includes a high-density reinforcement section, a medium-density support section and a low-density connection section, the high-density reinforcement section is located in the middle of the multi-filled pore bone plate structural skeleton, the medium-density support section is located on both sides of the high-density reinforcement section, and the low-density connection section is located on the outside of the medium-density support section; The structural skeleton of the bone plate with multiple filling pores is formed by interweaving silk threads, the density of the interweaving silk threads is unevenly distributed, and filling pores are formed between the interweaving silk threads, and the sizes of the filling pores are also unevenly distributed; The density of the silk threads interwoven on the skeleton of the multi-filled pore bone plate structure changes gradually, and the density of the silk threads interwoven on the skeleton of the multi-filled pore bone plate structure decreases gradually along the direction of the high-density reinforcement section, the medium-density support section and the low-density connection section. The size of the filled pores on the skeleton of the multi-filled pore bone plate structure also changes gradually, and the size of the filled pores increases gradually along the direction of the high-density reinforcement section, the medium-density support section and the low-density connection section; The filling pores are filled with polymer materials, and the exterior of the multi-filled pore bone fracture plate structure skeleton is coated with a layer of polymer materials; A plurality of fixing holes are arranged on the multi-filled pore bone fracture plate structure frame, and the plurality of fixing holes penetrate through the polymer material coated on the outside of the multi-filled pore bone fracture plate structure frame; A concave arc surface is provided on one side of the bone fracture plate.
[0009] Preferably, the number of the fixing holes is six, with one fixing hole respectively provided near the left and right sides of the high-density reinforcement section, and one fixing hole respectively provided at the middle position and near the outer side of the two medium-density support sections.
[0010] Preferably, the filling pores on the high-density reinforcement section are small square filling pores; The filling pores in the middle of the medium-density support section are small square filling pores, and the filling pores at the upper and lower sides of the medium-density support section are rectangular filling pores; The filling pores in the middle of the low-density connecting section are small square filling pores, and the filling pores in the upper and lower sides of the low-density connecting section are wide square filling pores; The width of the small square filled pores located in the middle of the low-density connecting section is smaller than the width of the small square filled pores located in the middle of the medium-density supporting section.
[0011] Preferably, the outer surfaces of the bone plates are smoothly transitioned through rounded corners.
[0012] A method for preparing the above-mentioned high-strength progressive bone fracture plate, preparing a reinforcement material and a matrix material, the reinforcement material is a polymer fiber material or a metal material, and the matrix material is a polymer material, and the preparation method comprises the following steps: Step (1): preparing the reinforcement material into a multi-filled pore bone plate structure skeleton; Step (2): placing the prepared multi-filled pore bone fracture plate structure skeleton and polymer material into a cavity mold respectively, and uniformly filling the polymer material into the filled pores of the multi-filled pore bone fracture plate structure skeleton by means of an oscillation method, and then press-forming the uniformly mixed materials through the cavity mold to obtain a progressive bone fracture plate semi-finished product after press-forming; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering. After sintering, a high-strength progressive bone plate is obtained.
[0013] Preferably, when the reinforcement material is titanium alloy wire and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing titanium alloy wires into a multi-filled pore titanium alloy bone plate structure skeleton by wire weaving; The diameter of the titanium alloy wire is 460 μm -520 μm, and the particle size of the polyetheretherketone powder is 350 μm -440 μm; The pore size of the high-density reinforcement section on the multi-filled porous titanium alloy bone plate structure skeleton is 250μm-350μm, the porosity is 15%-25%, the pore size of the medium-density support section is 370μm-450μm, the porosity is 27%-35%, and the pore size of the low-density connection section is 370-550μm, the porosity is 37%-45%; Step (2): placing the prepared multi-filled pore titanium alloy bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores of the multi-filled pore titanium alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 150MPa-220MPa, the pressure holding time is 24min-38min, after pressurization, a progressive bone plate semi-finished product is obtained; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, wherein the sintering method is hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature is 305°C-386°C, and the sintering time is 1.1h-1.7h. After sintering, a high-strength progressive bone plate is obtained.
[0014] Preferably, the diameter of the titanium alloy wire in step (1) is 500 μm, and the particle size of the polyetheretherketone powder is 400 μm; The pore size of the high-density reinforcement section in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section is 400 μm and the porosity is 30%, and the pore size of the low-density connection section is 500 μm and the porosity is 40%; The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes; The press forming method in step (2) is vacuum hot isostatic pressing, the press pressure is 200 MPa, and the holding time is 30 min; The sintering method in step (3) is vacuum hot isostatic pressing sintering, the sintering temperature is 345° C., and the sintering time is 1.5 h.
[0015] Preferably, when the reinforcement material is carbon fiber filaments and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing carbon fiber filaments into a multi-filled pore carbon fiber bone plate structure skeleton by filament weaving; The diameter of the carbon fiber filament is 8μm-13μm, the number of monofilaments is 6K-12K, and the particle size of the polyetheretherketone powder is 20μm-29μm; The pore size of the high-density reinforcement section on the multi-filled pore carbon fiber bone plate structure skeleton is 250μm-350μm, the porosity is 15%-25%, the pore size of the medium-density support section is 370μm-450μm, the porosity is 27%-35%, and the pore size of the low-density connection section is 370-550μm, the porosity is 37%-45%; Step (2): placing the prepared multi-filled pore carbon fiber bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores of the multi-filled pore carbon fiber bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 110MPa-190MPa, the pressure holding time is 22min-28min, after pressurization, a progressive bone plate semi-finished product is obtained; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 305°C-365°C, the sintering time being 0.6h-1.2h, and after sintering, a high-strength progressive bone plate is obtained.
[0016] Preferably, the diameter of the carbon fiber filament in step (1) is 10 μm, the number of monofilaments is 10K, and the particle size of the polyetheretherketone powder is 25 μm; The pore size of the high-density reinforcement section in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section is 400 μm and the porosity is 30%, and the pore size of the low-density connection section is 500 μm and the porosity is 40%; The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes; The press forming method in step (2) is vacuum cold isostatic pressing, the press pressure is 160 MPa, and the holding time is 25 min; The sintering method in step (3) is spark plasma sintering, the sintering temperature is 343° C., and the sintering time is 1 h.
[0017] Preferably, the reinforcement material may also be a degradable metal material.
[0018] The beneficial effects of the present invention are: 1. By setting three density segments on the bone plate, the actual positions of the three density segments can be adjusted according to the different locations of the patient's bone injury. The biomechanical properties of the bone plate can be optimized by adjusting the porosity and pore size of different parts of the bone plate. On the one hand, the bone plate provides biomechanical internal fixation for the bone tissue at the implantation site, and at the same time, it can ensure that the bone tissue is subjected to sufficient stress stimulation, stimulate the self-repair function of the bone tissue, and achieve mechanical compatibility between the bone plate and the human bone tissue. At the same time, it can save materials and reduce production costs.
[0019] Among them, the high-density reinforced section is the location where the contact bone damage is most serious and the location where the plate is subjected to the greatest force. The aperture and porosity specification parameters can ensure the high strength of the central part of the plate where the force is greatest, and achieve the mechanical support of the plate through sufficient strength. If it is lower than this parameter range, the central part of the plate is prone to breakage during actual use.
[0020] The pore size and porosity specification parameters of the medium-density support segment can provide good auxiliary support for the area around the bone injury site. At the same time, they can assist in the fixation of the high-density reinforcement segment, increase the stability of the high-density reinforcement segment fixation, and prevent the area around the bone injury site from being interfered with by stress and causing secondary damage.
[0021] The low-density connecting section adopts relatively large pore size and porosity because when the bone plate is actually subjected to stress, the stress on both sides is relatively small. This range matches the actual load-bearing capacity, avoiding the stress shielding effect while preventing the bone plate from loosening after long-term use.
[0022] 2. The bone plate is prepared into a multi-filled pore bone plate structure skeleton by using a reinforcement material, and then the multi-filled pore bone plate structure skeleton and the matrix material are uniformly filled and mixed by ultrasonic vibration, and then the mixed material is pressurized by vacuum hot isostatic pressing or vacuum cold isostatic pressing process, and finally the molded material is placed in a high-temperature oven for sintering; It can be clearly seen that each of the steps can play a role in increasing the strength of the bone plate. After the overall steps are completed, the strength of the bone plate is significantly increased. Therefore, the bone plate can withstand higher load impact forces when in use, and avoid a series of quality problems such as breakage and fragmentation of the bone plate during use to the greatest extent. It greatly improves the overall mechanical properties of the bone plate and ensures that the bone plate can be used stably for a long time.
[0023] 3. The finished bone plate made of degradable metal materials has obvious bone induction ability. Specifically, the degradable metal materials used in the finished bone plate, such as degradable zinc alloy and degradable magnesium alloy, will react with the body fluids in the human body to produce Mg ions and Zn ions. These two ions can promote bone regeneration through three main strategies, including balancing osteoblasts and osteoclasts, regulating the immune microenvironment, and promoting bone angiogenesis, thereby achieving bone induction effect and effectively accelerating the recovery of the fracture site.
[0024] 4. The bone plate is made by mixing biodegradable metal materials and medical plastics. Compared with the traditional metal material, its overall weight is lighter. After the weight is reduced, it can significantly reduce the patient's bone loss and avoid a series of chain symptoms such as osteoporosis and bone calcification. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a stereoscopic view of a finished product of a bone fracture plate of the present invention; Figure 2 is another stereoscopic view of the finished product of the bone plate of the present invention; Figure 3 It is a three-dimensional diagram of the structural skeleton of the multi-filled pore bone fracture plate of the present invention; Figure 4 The present invention Figure 3 Enlarged view of point A in the middle.
[0027] Explanation of symbols in the figure 1. High-density reinforcement section; 2. Medium-density support section; 3. Low-density connection section; 4. Fixing hole; 5. Concave arc surface; 6. Multi-filled pore bone plate structure skeleton; 7. Rounded corners; 8. Silk thread; 9. Filled pores. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with embodiments.
[0030] pass Figure 1-Figure 4It can be seen that the high-strength progressive bone plate is provided with a multi-filled pore bone plate structural skeleton 6, which includes a high-density reinforcement section 1, a medium-density support section 2 and a low-density connection section 3. The high-density reinforcement section 1 is located in the middle position of the multi-filled pore bone plate structural skeleton 6, the medium-density support section 2 is located on both sides of the high-density reinforcement section 1, and the low-density connection section 3 is located on the outside of the medium-density support section 2.
[0031] The multi-filled pore bone plate structural skeleton 6 is formed by interweaving threads 8, the density of the interwoven threads 8 is unevenly distributed, and filled pores 9 are formed between the interwoven threads 8, and the sizes of the filled pores 9 are also unevenly distributed.
[0032] The density of the interwoven threads 8 on the multi-filled pore plate structure skeleton 6 changes gradually, and the density of the interwoven threads 8 on the multi-filled pore plate structure skeleton 6 decreases gradually along the direction of the high-density reinforcement section 1, the medium-density support section 2 and the low-density connection section 3.
[0033] The sizes of the filling pores 9 on the multi-filling pore bone plate structural skeleton 6 also change gradually, and the sizes of the filling pores 9 increase gradually along the directions of the high-density reinforcement section 1, the medium-density support section 2 and the low-density connection section 3.
[0034] In actual use, the position of the high-density reinforced section 1 is the location where the contact bone damage is most serious and the location where the plate is subjected to the greatest force. The aperture and porosity specification parameters can ensure the high strength of the center part of the plate where the force is greatest, and achieve the mechanical support of the plate through sufficient strength. If it is lower than this parameter range, the center part of the plate is prone to breakage during actual use.
[0035] The pore size and porosity specification parameters of the medium-density support segment 2 can provide good auxiliary support for the area around the bone injury site. At the same time, they can assist in the fixation of the high-density reinforcement segment 1, increase the stability of the fixation of the high-density reinforcement segment 1, and prevent the area around the bone injury site from being interfered with by stress and causing secondary damage.
[0036] The low-density connecting section 3 adopts relatively large pore size and porosity because when the bone plate is actually subjected to stress, the stress on both sides is relatively small. This range matches the actual load-bearing capacity, avoiding the stress shielding effect while preventing the bone plate from loosening after long-term use.
[0037] In short, by setting three density segments, the actual positions of the three density segments can be adjusted according to the different locations of the patient's bone injury. The biomechanical properties of the plate can be optimized by adjusting the porosity and pore size of different parts of the plate. On the one hand, the plate provides biomechanical internal fixation for the bone tissue at the implantation site, and on the other hand, it can ensure that the bone tissue is subjected to sufficient stress stimulation, stimulate the self-repair function of the bone tissue, and achieve mechanical compatibility between the plate and the human bone tissue. At the same time, it can save materials and reduce production costs.
[0038] The filling pores 9 are filled with polymer materials, and the exterior of the multi-filled pore bone fracture plate structural framework 6 is coated with a layer of polymer materials.
[0039] A plurality of fixing holes 4 are arranged on the multi-filled pore bone fracture plate structure skeleton 6 , and the plurality of fixing holes 4 penetrate through the polymer material coated on the outside of the multi-filled pore bone fracture plate structure skeleton 6 .
[0040] The surface of one side of the bone plate is provided with a concave arc surface 5. The shape of the concave arc surface 5 can better adapt to the anatomical structure of the human skeleton, so that the bone plate can better fit the human skeleton. The curvature of the concave surface 5 is the same as the curvature of the damaged bone, which can further promote the anatomical reduction of the bone and achieve a better fixation effect.
[0041] A plurality of fixing holes 4 are respectively arranged at the positions of the high-density reinforcement section and the medium-density support section.
[0042] The filling pores 9 on the high-density reinforcement section 1 are small square filling pores, the filling pores 9 in the middle position on the medium-density support section 2 are small square filling pores, the filling pores 9 at the upper and lower sides of the medium-density support section are rectangular filling pores, the filling pores 9 in the middle position on the low-density connecting section 3 are small square filling pores, and the filling pores 9 at the upper and lower sides of the low-density connecting section 3 are wide square filling pores.
[0043] The width of the small squares filling the pores in the middle of the low-density connecting section 3 is smaller than the width of the small squares filling the pores in the middle of the medium-density supporting section 2 .
[0044] There are six fixing holes 4 . One fixing hole 4 is provided near the left and right sides of the high-density reinforcement section 1 . One fixing hole 4 is provided in the middle and near the outer sides of the two medium-density support sections 2 .
[0045] The distribution of the fixing holes 4 can ensure that both sides and the middle of the bone plate are effectively fixed, thereby increasing the overall fixation stability of the bone plate.
[0046] Specifically, fixing holes 4 are arranged on the high-density reinforcement segment 1 near the left and right sides, in the middle of the two medium-density support segments 2, and near the outer sides, so as to ensure that the high-density reinforcement segment 1 and the medium-density support segment 2 can be fully fixed. In addition, since the low-density connection segment 3 mainly serves as an auxiliary fixation, the fixing holes 4 near the outer sides of the medium-density support segment 2 can also play an auxiliary supporting and fixing role for the low-density connection segment 3, thereby ensuring that each position is effectively fixed when the bone plate is fixed.
[0047] The number of fixing holes 4 should not be too many. If there are too many fixing holes 4, more holes will be drilled into the bone, the periosteum will be peeled off in a larger area, and the bone will be damaged more. Moreover, if there are too many fixing holes 4, the spacing between adjacent fixing holes 4 will become smaller, and the curvature between adjacent fixing holes 4 will become smaller. During surgery, the bone plate cannot fit tightly against the bone, resulting in compression of the periosteum by the bone plate, which is not conducive to effective healing of the fracture site.
[0048] The hole diameter of the fixing hole 4 is not less than 1 / 4 of the width of the bone plate. If the outer diameter of the fixing hole 4 is less than 1 / 4 of the width of the bone plate, the locking area of the fixing screw on the bone plate becomes smaller, which will cause the bone plate to be loosely fixed, uneven stress distribution, and even cause secondary injury to the damaged bone.
[0049] The outer surface of the bone plate is provided with rounded corners 7. By providing the rounded corners 7, it is possible to prevent the bone tissue surface from being damaged after the bone plate is fixed.
[0050] A method for preparing the above-mentioned high-strength progressive bone fracture plate, preparing a reinforcement material and a matrix material, the reinforcement material is a polymer fiber material or a metal material, and the matrix material is a polymer material, and the preparation method comprises the following steps: Step (1): preparing the reinforcement material into a multi-filled pore bone plate structure skeleton 6.
[0051] Step (2): Place the prepared multi-filled pore bone fracture plate structure skeleton 6 and polymer material into the cavity mold respectively, and use an oscillation method to evenly fill the polymer material into the filling pores 9 of the multi-filled pore bone fracture plate structure skeleton 6, and then press-form the evenly mixed materials through the cavity mold to obtain a progressive bone fracture plate semi-finished product after press-forming.
[0052] Vacuum cold isostatic pressing is often used for powders that are difficult to press, such as hard metals.
[0053] Vacuum hot isostatic pressing is mainly used for the molding of high-performance powder material products, such as the industrial production of powder metallurgy high-temperature alloys, powder metallurgy high-speed steel, carbon materials, ceramic materials, etc.
[0054] Oscillation methods include ultrasonic oscillation and mechanical oscillation. The difference between the two is that the uniformity of ultrasonic oscillation is higher than that of mechanical oscillation. When the mixing accuracy requirement is high, ultrasonic oscillation is usually used, while mechanical oscillation is used instead.
[0055] Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering. After sintering, a high-strength progressive bone plate is obtained.
[0056] Example 1 When the reinforcement material is titanium alloy wire and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing titanium alloy wires into a multi-filled pore titanium alloy bone plate structural skeleton by wire weaving.
[0057] The diameter of the titanium alloy wire is 460 μm-520 μm, and the particle size of the polyetheretherketone powder is 350 μm-440 μm.
[0058] The pore size of the high-density reinforcement segment on the multi-filled porous titanium alloy bone plate structure skeleton is 250μm-350μm, and the porosity is 15%-25%, the pore size of the medium-density support segment is 370μm-450μm, and the porosity is 27%-35%, and the pore size of the low-density connection segment is 370-550μm, and the porosity is 37%-45%.
[0059] Step (2): placing the prepared multi-filled pore titanium alloy bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores 9 of the multi-filled pore titanium alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 150MPa-220MPa, the pressure holding time is 24min-38min, after pressurization, a progressive bone plate semi-finished product is obtained.
[0060] Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, wherein the sintering method is hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature is 305°C-386°C, and the sintering time is 1.1h-1.7h. After sintering, a high-strength progressive bone plate is obtained.
[0061] In Example 1, the diameter of the titanium alloy wire in step (1) is 500 μm, and the particle size of the polyetheretherketone powder is 400 μm.
[0062] The pore size of the high-density reinforcement section in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section is 400 μm and the porosity is 30%, and the pore size of the low-density connection section is 500 μm and the porosity is 40%.
[0063] The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes.
[0064] The pressure forming method in step (2) is vacuum hot isostatic pressing, the pressure is 200 MPa, and the holding time is 30 minutes.
[0065] The sintering method in step (3) is vacuum hot isostatic pressing sintering, the sintering temperature is 345° C., and the sintering time is 1.5 h.
[0066] Titanium alloy material has good corrosion resistance, biocompatibility, superior mechanical properties and fatigue resistance. It has good wear resistance in the assembly and can effectively improve the mechanical properties of polyetheretherketone material and ensure the strength of the bone plate.
[0067] Example 2 When the reinforcement material is carbon fiber filaments and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing carbon fiber filaments into a multi-filled pore carbon fiber bone plate structural skeleton by filament weaving.
[0068] The diameter of the carbon fiber filament is 8μm-13μm, the number of single filaments is 6K-12K, and the particle size of the polyetheretherketone powder is 20μm-29μm.
[0069] The pore size of the high-density reinforcement section on the multi-filled porous carbon fiber bone plate structure skeleton is 250μm-350μm, and the porosity is 15%-25%, the pore size of the medium-density support section is 370μm-450μm, and the porosity is 27%-35%, and the pore size of the low-density connection section is 370-550μm, and the porosity is 37%-45%.
[0070] Step (2): placing the prepared multi-filled pore carbon fiber bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores 9 of the multi-filled pore carbon fiber bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 110MPa-190MPa, the pressure holding time is 22min-28min, after pressurization, a progressive bone plate semi-finished product is obtained.
[0071] Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 305°C-365°C, the sintering time being 0.6h-1.2h, and after sintering, a high-strength progressive bone plate is obtained.
[0072] Among them, hot pressing sintering refers to the sintering process of accelerating the flow, rearrangement and densification of materials under a certain external force (depending on the strength of the mold material, the general pressure is 10-40MPa). The temperature required for hot pressing sintering is 100-150℃ lower than that of normal pressure sintering, but the driving force of hot pressing sintering is 20-100 times greater than that of normal pressure sintering.
[0073] Hot pressing sintering can obtain better mechanical properties of materials, and can reduce sintering time or lower sintering temperature, reduce the amount of covalent bond ceramic sintering aids, thereby improving the high temperature mechanical properties of materials.
[0074] The basic principle of vacuum hot isostatic pressing sintering is to use high-pressure gas as a pressure medium to act on the material (including encapsulated powder, green billet or sintered body), so that it is subjected to isotropic pressure during the heating process, and the material is densified by the combined effect of high temperature and high pressure.
[0075] The use of vacuum hot isostatic pressing sintering can reduce the sintering temperature and shorten the sintering time. At the same time, it can greatly reduce or even eliminate the use of sintering aids, improve ceramic performance and reliability, and is particularly suitable for manufacturing products with complex shapes.
[0076] Gas pressure sintering refers to applying a certain gas pressure during high temperature sintering, and the pressure range is usually 1-10MPa, in order to inhibit the decomposition and weight loss of materials at high temperatures, thereby increasing the sintering temperature and further promoting the densification of materials to obtain high-density products. Gas pressure sintering and vacuum hot isostatic pressing sintering both use gas as a method of transmitting pressure.
[0077] Compared with hot pressing sintering and vacuum hot isostatic pressing sintering, the biggest advantage of gas pressure sintering is that it can reduce investment costs, has better preparation performance, is suitable for products with complex shapes, and realizes mass production.
[0078] Microwave sintering is often used for the sintering of ceramic materials. The dielectric loss of ceramic materials in the microwave electromagnetic field is used to make the materials reach the sintering temperature, thereby achieving the sintering and densification of ceramics.
[0079] Spark plasma sintering, also known as "plasma activated sintering", is a new material preparation technology that achieves material sintering through thermal effects or other field effects by directly applying large pulse currents in molds or samples.
[0080] Spark plasma sintering can ensure uniformity of heating temperature, fast heating rate, low sintering temperature, short sintering time, high production efficiency, fine and uniform product structure, and can maintain the natural state of raw materials. It can obtain high-density materials and is often used in sintering gradient materials and complex workpieces.
[0081] Solid-state metal sintering is a sintering process achieved by using powdered materials. Powdered materials can be molded into the desired shape to produce parts with complex shapes and sophisticated designs. In addition, solid-state sintering can improve the mechanical properties of materials. Compared with traditional processes, solid-state sintering has a shorter cycle time, which means that the sintering process can be completed in a few minutes instead of hours or longer. This high productivity and rapid material development capabilities make solid-state metal sintering more widely used.
[0082] More importantly, solid metal sintering can be carried out at lower temperatures than traditional sintering processes, which is very advantageous because it helps to minimize energy consumption and reduce the risk of thermal damage to the sintered material. At the same time, solid metal sintering is an extremely versatile process. It can be used for densification sintering of low-melting-point metals, ultra-high temperature ceramics, and even for bonding dissimilar materials that require uneven temperatures. In addition, solid sintering can also be used to sinter porous components and fully dense components, and has a wide range of applications.
[0083] In summary, solid-state metal sintering offers a variety of advantages, including the ability to produce complex shapes, better mechanical properties, shorter sintering times, lower sintering temperatures, versatility, high-precision process control, and cost-effectiveness, which make solid-state sintering an ideal manufacturing method for a wide range of applications.
[0084] In Example 2, the diameter of the carbon fiber filaments in step (1) is 10 μm, the number of single filaments is 10K, and the particle size of the polyetheretherketone powder is 25 μm.
[0085] The pore size of the high-density reinforcement section in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section is 400 μm and the porosity is 30%, and the pore size of the low-density connection section is 500 μm and the porosity is 40%.
[0086] The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes.
[0087] The pressure forming method in step (2) is vacuum cold isostatic pressing, the pressure is 160 MPa, and the holding time is 25 min.
[0088] The sintering method in step (3) is spark plasma sintering, the sintering temperature is 343° C., and the sintering time is 1 h.
[0089] Carbon fiber materials have the characteristics of high strength and low modulus, which can not only ensure the strength of the bone plate, but also avoid the problem of stress shielding effect caused by high elastic modulus in traditional metal material preparation.
[0090] The fixing hole 4 is formed by hot extrusion or hot forming.
[0091] Existing bone plate fixation holes are usually machined, but machining holes will destroy the continuity of the reinforcement structure and affect the mechanical properties around the holes. Hot extrusion or hot forming can effectively ensure the continuity of the reinforcement around the holes, thereby ensuring the mechanical properties around the holes.
[0092] The reinforcement material may also be made of degradable metal materials, which include degradable zinc alloy wires, degradable zinc alloy powders, degradable magnesium alloy wires or degradable magnesium alloy powders.
[0093] Degradable metal materials will react with body fluids in the human body and be gradually corroded and degraded by the body fluids. For example, when using degradable zinc alloy wire or degradable magnesium alloy wire, magnesium ions or zinc ions will be produced when the degradable zinc alloy wire or degradable magnesium alloy wire reacts with body fluids. The two ions will be released from the fixation holes of the bone plate. These two ions, as the most important trace elements in bone tissue and as indispensable active ingredients in human biological activities, play an important role in bone tissue repair and can effectively accelerate the recovery of the fracture site.
[0094] Example 3 When the reinforcement material is titanium alloy powder and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing titanium alloy powder into a multi-filled porous titanium alloy bone plate structure skeleton by 3D printing.
[0095] The particle size of the titanium alloy powder is 80 μm-120 μm, and the particle size of the polyetheretherketone powder is 120 μm-290 μm.
[0096] The pore size of the high-density reinforcement section 1 on the multi-filled porous titanium alloy bone plate structure skeleton is 250μm-350μm, and the porosity is 15%-25%, the pore size of the medium-density support section 2 is 370μm-450μm, and the porosity is 27%-35%, and the pore size of the low-density connection section 3 is 370-550μm, and the porosity is 37%-45%.
[0097] Step (2): placing the prepared multi-filled pore titanium alloy bone plate structure skeleton into the cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores 9 of the multi-filled pore titanium alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, and the shaking time is 22min-39min.
[0098] The difference between ultrasonic oscillation and mechanical oscillation is that the uniformity of ultrasonic oscillation is higher than that of mechanical oscillation. When the mixing accuracy requirement is high, ultrasonic oscillation is usually used, while mechanical oscillation is used instead.
[0099] After uniform filling, the mixed material is pressurized through a cavity mold by vacuum hot isostatic pressing or vacuum cold isostatic pressing. The pressurization pressure is 150MPa-260MPa, and the holding time is 16min-26min. After pressurization, a progressive bone plate semi-finished product is obtained.
[0100] Step (3): placing the progressive bone plate forming material into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 280°C-420°C, the sintering time being 1.6 h-2.4 h, and after sintering, a high-strength progressive bone plate is obtained.
[0101] In Example 3, the particle size of the titanium alloy powder in step (1) is 100 μm, and the particle size of the polyetheretherketone powder is 200 μm.
[0102] The pore size of the high-density reinforcement section 1 in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section 2 is 400 μm and the porosity is 30%, and the pore size of the low-density connection section 3 is 500 μm and the porosity is 40%.
[0103] The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes.
[0104] The pressure forming method in step (2) is vacuum hot isostatic pressing, the pressure is 200 MPa, and the holding time is 20 minutes.
[0105] The sintering method in step (3) is vacuum hot isostatic pressing sintering, the sintering temperature is 350° C., and the sintering time is 2 h.
[0106] Example 4 When the reinforcement material is a degradable zinc alloy wire and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing the degradable zinc alloy wire into a multi-filled pore degradable zinc alloy bone plate structure skeleton by wire weaving.
[0107] The diameter of the degradable zinc alloy wire is 520 μm-620 μm, and the particle size of the polyetheretherketone powder is 400 μm-520 μm.
[0108] The pore size of the high-density reinforcement segment 1 on the multi-filled porous biodegradable zinc alloy bone plate structure skeleton is 250μm-350μm, and the porosity is 15%-25%, the pore size of the medium-density support segment 2 is 370μm-450μm, and the porosity is 27%-35%, and the pore size of the low-density connection segment 3 is 370-550μm, and the porosity is 37%-45%.
[0109] Step (2): placing the prepared multi-filled porous degradable zinc alloy bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores 9 of the porous zinc alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 22min-32min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 80MPa-110MPa, the pressure holding time is 12min-18min, after pressurization, a progressive bone plate semi-finished product is obtained.
[0110] Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 330°C-385°C, the sintering time being 0.8h-1.2h, and after sintering, a high-strength and degradable progressive bone plate is obtained.
[0111] In Example 4, the diameter of the degradable zinc alloy wire in step (1) is 560 μm, and the particle size of the polyetheretherketone powder is 450 μm.
[0112] The pore size of the high-density reinforcement section 1 in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section 2 is 400 μm and the porosity is 30%, and the pore size of the low-density connection section 3 is 500 μm and the porosity is 40%.
[0113] The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes.
[0114] The press molding method in step (2) is vacuum cold isostatic pressing, the press pressure is 100 MPa, and the holding time is 15 minutes.
[0115] The sintering method in step (3) is hot pressing sintering, the sintering temperature is 350° C., and the sintering time is 1 h.
[0116] Example 5 When the reinforcement material is a degradable magnesium alloy wire and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing the degradable magnesium alloy wire into a multi-filled pore degradable magnesium alloy bone plate structure skeleton by wire weaving.
[0117] The diameter of the degradable magnesium alloy wire is 580 μm-720 μm, and the particle size of the polyetheretherketone powder is 430 μm-590 μm.
[0118] The pore size of the high-density reinforcement segment 1 on the multi-filled porous biodegradable magnesium alloy bone plate structure skeleton is 250μm-350μm, and the porosity is 15%-25%, the pore size of the medium-density support segment 2 is 370μm-450μm, and the porosity is 27%-35%, and the pore size of the low-density connection segment 3 is 370-550μm, and the porosity is 37%-45%.
[0119] Step (2): placing the prepared multi-filled porous degradable magnesium alloy bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores 9 of the porous magnesium alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26 min-33 min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 120 MPa-190 MPa, the pressure holding time is 3 min-9 min, after pressurization, a progressive bone plate semi-finished product is obtained. Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 280°C-420°C, the sintering time being 0.6h-1.2h, and after sintering, a high-strength and degradable progressive bone plate is obtained.
[0120] In Example 5, the diameter of the degradable magnesium alloy wire in step (1) is 680 μm, and the particle size of the polyetheretherketone powder is 500 μm.
[0121] The pore size of the high-density reinforcement section 1 in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support section 2 is 400 μm and the porosity is 30%, and the pore size of the low-density connection section 3 is 500 μm and the porosity is 40%.
[0122] The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes.
[0123] The pressure forming method in step (2) is vacuum hot isostatic pressing, the pressure is 150 MPa, and the holding time is 5 minutes.
[0124] The sintering method in step (3) is solid metal sintering, the sintering temperature is 330° C., and the sintering time is 1 h.
[0125] The multi-filled porous bone plate structural skeleton is prepared into a progressive structural form by using 3D printing or wire weaving to form a reinforcing material. It is an integrated three-dimensional process with a stable structure and high compressive strength. It effectively solves the problem that the reinforcing material in the existing bone plate is evenly distributed in the polyetheretherketone matrix in the form of a prepreg tape, and the interface bonding force between the two is low. When applied to parts of the human body with higher bearing capacity, the bone plate is prone to technical problems such as breakage and delamination.
[0126] The preparation process of the bone plate is to use common medical metal materials, polymer fiber materials or degradable metal materials to prepare a multi-filled porous bone plate structure skeleton, and then uniformly fill and mix the multi-filled porous bone plate structure skeleton and the matrix material by ultrasonic vibration, and then form them by isostatic pressing after mixing, and finally put the formed material into a high-temperature oven for sintering.
[0127] It can be clearly seen that each of the steps can play a role in increasing the strength of the bone plate. After the overall steps are completed, the strength of the bone plate is significantly enhanced. Therefore, the bone plate can withstand higher load impact forces when in use, and avoid a series of quality problems such as breakage and fragmentation of the bone plate during use to the greatest extent. The overall mechanical properties of the bone plate are greatly improved, ensuring that the bone plate can be used stably for a long time.
[0128] Moreover, by using degradable metal materials as reinforcement materials, the finished bone plate produced by the preparation method has obvious bone induction ability. Specifically, the degradable metal materials used in the finished bone plate, such as degradable zinc alloy and degradable magnesium alloy, will react with body fluids in the human body to produce Mg ions and Zn ions. These two ions can promote bone regeneration through three main strategies, including balancing osteoblasts and osteoclasts, regulating the immune microenvironment, and promoting bone angiogenesis, ultimately achieving a bone induction effect.
[0129] More importantly, the bone plate prepared by the preparation method is prepared by mixing different types of reinforcement materials and matrix materials. For example, the reinforcement material is a degradable metal wire or a degradable metal powder. Each reinforcement material and the corresponding matrix material have fixed preparation parameter values, such as the diameter and particle size of the reinforcement material, the particle size of the matrix material, and the pore size and porosity of different density segments in the prepared multi-filled porous bone plate structure skeleton.
[0130] The selected reinforcement material and matrix material are subjected to preparation processes such as uniform mixing, pressure molding, and sintering to obtain a high-strength progressive bone plate. In addition, the above preparation processes have strict and specific preparation parameters and preparation processes, such as the pressure molding method, the sintering method during the sintering process, the sintering temperature and the sintering time, etc. The above preparation parameters and preparation processes are the key to preparing the finished high-strength progressive bone plate material.
[0131] Secondly, this high-strength progressive bone plate is made by mixing biodegradable metal materials and medical plastics. Compared with traditional bone plates made of metal materials, its overall weight is lighter. After the weight is reduced, it can significantly reduce the patient's bone loss and avoid a series of chain symptoms such as osteoporosis and bone calcification.
[0132] However, what is described above is only a specific embodiment of the present invention and should not be used to limit the scope of implementation of the present invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the scope of protection of the present invention should still fall within the scope covered by the claims of the present invention.
Claims
1. A high-strength progressive bone plate, Its characteristics are: A multi-filled pore bone fracture plate structure skeleton is provided, the multi-filled pore bone fracture plate structure skeleton comprises a high-density reinforcement section, a medium-density support section and a low-density connection section, the high-density reinforcement section is located in the middle of the multi-filled pore bone fracture plate structure skeleton, the medium-density support section is located on both sides of the high-density reinforcement section, and the low-density connection section is located on the outside of the medium-density support section; The multi-filling pore bone fracture plate structural skeleton is formed by interweaving silk threads, the density of the interweaving silk threads is unevenly distributed, and filling pores are formed between the interweaving silk threads, and the sizes of the filling pores are also unevenly distributed; The density of the interwoven threads on the multi-filled pore bone fracture plate structure skeleton changes gradually, and the density of the interwoven threads on the multi-filled pore bone fracture plate structure skeleton decreases gradually along the direction of the high-density reinforcement section, the medium-density support section and the low-density connection section; The size of the filled pores on the multi-filled pore bone fracture plate structure skeleton also changes gradually, and the size of the filled pores increases gradually along the direction of the high-density reinforcement section, the medium-density support section and the low-density connection section; The filling pores are filled with polymer materials, and the exterior of the multi-filling pore bone fracture plate structure skeleton is coated with a layer of polymer materials; The multi-filled pore bone fracture plate structure skeleton is provided with a plurality of fixing holes, and the plurality of fixing holes penetrate through the polymer material coated on the outside of the multi-filled pore bone fracture plate structure skeleton; A concave arc surface is provided on one side of the bone fracture plate.
2. The high-strength progressive bone plate according to claim 1, Features: The filling pores on the high-density reinforcement section are small square filling pores; The filling pores located in the middle of the medium-density support segment are small square filling pores, and the filling pores located at the upper and lower sides of the medium-density support segment are rectangular filling pores; The filling pores located in the middle of the low-density connecting section are small square filling pores, and the filling pores located at the upper and lower sides of the low-density connecting section are wide square filling pores; The width of the small square filled pores located in the middle of the low-density connecting section is smaller than the width of the small square filled pores located in the middle of the medium-density supporting section.
3. The high-strength progressive bone plate according to claim 1, Features: The number of the fixing holes is six. A fixing hole is provided near the left and right sides of the high-density reinforcement section, and a fixing hole is provided in the middle position and near the outer side of the two medium-density support sections.
4. The high-strength progressive bone plate according to claim 1, Features: The outer surfaces of the bone fracture plates are smoothly transitioned through rounded corners.
5. A method for preparing the high-strength progressive bone plate according to any one of claims 1 to 4, Features: Prepare a reinforcement material and a matrix material, wherein the reinforcement material is a polymer fiber material or a metal material, and the matrix material is a polymer material. The preparation method comprises the following steps: Step (1): preparing the reinforcement material into a multi-filled pore bone plate structure skeleton; Step (2): placing the prepared multi-filled pore bone fracture plate structure skeleton and polymer material into a cavity mold respectively, and uniformly filling the polymer material into the filled pores of the multi-filled pore bone fracture plate structure skeleton by means of an oscillation method, and then press-forming the uniformly mixed materials through the cavity mold to obtain a progressive bone fracture plate semi-finished product after press-forming; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering. After sintering, a high-strength progressive bone plate is obtained.
6. The method for preparing the high-strength progressive bone plate according to claim 5, Features: When the reinforcement material is titanium alloy wire and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing titanium alloy wires into a multi-filled pore titanium alloy bone plate structure skeleton by wire weaving; The diameter of the titanium alloy wire is 460 μm-520 μm, and the particle size of the polyetheretherketone powder is 350 μm-440 μm; The high-density reinforcement section on the multi-filled porous titanium alloy bone plate structure skeleton has a pore size of 250 μm-350 μm and a porosity of 15%-25%, a medium-density support section has a pore size of 370 μm-450 μm and a porosity of 27%-35%, and a low-density connection section has a pore size of 370-550 μm and a porosity of 37%-45%; Step (2): placing the prepared multi-filled pore titanium alloy bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores of the multi-filled pore titanium alloy bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 150MPa-220MPa, the pressure holding time is 24min-38min, after pressurization, a progressive bone plate semi-finished product is obtained; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, wherein the sintering method is hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature is 305°C-386°C, and the sintering time is 1.1h-1.7h. After sintering, a high-strength progressive bone plate is obtained.
7. The method for preparing the high-strength progressive bone plate according to claim 5, Features: When the reinforcement material is carbon fiber filaments and the matrix material is polyetheretherketone powder, the preparation method comprises the following steps: Step (1): preparing the carbon fiber wire into a multi-filled pore carbon fiber bone plate structure skeleton by wire weaving; The diameter of the carbon fiber filament is 8 μm-13 μm, the number of monofilaments is 6K-12K, and the particle size of the polyetheretherketone powder is 20 μm-29 μm; The high-density reinforcement section on the multi-filled pore carbon fiber bone plate structural skeleton has a pore size of 250 μm-350 μm and a porosity of 15%-25%, the medium-density support section has a pore size of 370 μm-450 μm and a porosity of 27%-35%, and the low-density connection section has a pore size of 370-550 μm and a porosity of 37%-45%; Step (2): placing the prepared multi-filled pore carbon fiber bone plate structure skeleton into a cavity mold, and then filling the cavity mold with polyetheretherketone powder, the filling method adopts multiple equal fillings, after each filling is completed, the polyetheretherketone powder is evenly filled into the filling pores of the multi-filled pore carbon fiber bone plate structure skeleton by shaking, the shaking method is mechanical shaking or ultrasonic shaking, the shaking time is 26min-33min, after uniform filling, the mixed material is pressurized by the cavity mold, the pressurization method is vacuum hot isostatic pressing or vacuum cold isostatic pressing, the pressurization pressure is 110MPa-190MPa, the pressure holding time is 22min-28min, after pressurization, a progressive bone plate semi-finished product is obtained; Step (3): placing the semi-finished progressive bone plate into a high-temperature oven for sintering, the sintering method being hot pressing sintering, vacuum hot isostatic pressing sintering, gas pressure sintering, microwave sintering, spark plasma sintering or solid metal sintering, the sintering temperature being 305°C-365°C, the sintering time being 0.6h-1.2h, and after sintering, a high-strength progressive bone plate is obtained.
8. The method for preparing the high-strength progressive bone plate according to claim 6, Features: The diameter of the titanium alloy wire in step (1) is 500 μm, and the particle size of the polyetheretherketone powder is 400 μm; The pore size of the high-density reinforcement segment in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support segment is 400 μm and the porosity is 30%, and the pore size of the low-density connection segment is 500 μm and the porosity is 40%; The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes; The press forming method in step (2) is vacuum hot isostatic pressing, the press pressure is 200 MPa, and the holding time is 30 min; The sintering method in step (3) is vacuum hot isostatic pressing sintering, the sintering temperature is 345° C., and the sintering time is 1.5 h.
9. The method for preparing the high-strength progressive bone plate according to claim 7, Features: The diameter of the carbon fiber filament in step (1) is 10 μm, the number of single filaments is 10K, and the particle size of the polyetheretherketone powder is 25 μm; The pore size of the high-density reinforcement segment in step (1) is 300 μm and the porosity is 20%, the pore size of the medium-density support segment is 400 μm and the porosity is 30%, and the pore size of the low-density connection segment is 500 μm and the porosity is 40%; The shaking method in step (2) is ultrasonic shaking, and the shaking time is 30 minutes; The pressurization method in step (2) is vacuum cold isostatic pressing, the pressurization pressure is 160 MPa, and the holding time is 25 min; The sintering method in step (3) is spark plasma sintering, the sintering temperature is 343° C., and the sintering time is 1 hour.
10. The method for preparing the high-strength progressive bone plate according to claim 5, Features: The reinforcement material may also be a degradable metal material.
Citation Information
Patent Citations
Absorbable bone-repairing material and preparation method thereof
CN106178122A
Bone plate and manufacturing method thereof
CN106267380A
Gradient and porous magnesium alloy material used for bone defect repair
CN107190190A
Multi-pore bionic skull repair material and individualized manufacturing method
CN108273137A
Artificial bone with bionic light structure and preparation method of artificial bone
CN117162538A