Nanoscale zirconia ceramic implant and preparation method thereof
By forming a surface treatment layer and a bioactive molecule layer on the zirconia ceramic implant, and using fixed connectors, the problem of insufficient bioactivity and compatibility of zirconia ceramic implants in the dental field is solved, and its mechanical properties are improved. performance and stability, achieving better bone tissue integration and long-term application effects.
Patent Information
- Application Number
- CN202410978055.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
Existing zirconia ceramic implants have problems such as poor biological activity, insufficient tissue compatibility and weak interface adhesion in dental applications, which limits their application potential.
Nanoscale zirconia ceramic implants are used to form a surface treatment layer and a bioactive molecular layer on the matrix, and fixed connectors are used to fix the implants in bone tissue to improve their biocompatibility and mechanical properties.
It improves the biocompatibility, mechanical strength, bioactivity and wear resistance of the implant, prolongs its service life, and enhances the bonding force with bone tissue to ensure the stability and safety of the implant.
Abstract
Description
Technical Field
[0001] The invention relates to the field of medical ceramic materials, and in particular to a nano-scale zirconium oxide ceramic implant and a preparation method thereof. Background Art
[0002] An implant is a medical prosthesis that is usually implanted into the body through surgery to replace missing tissues or organs. Implants are increasingly used in the oral field, such as for dental implants and bone replacement materials. Zirconia ceramics is a commonly used implant material with the advantages of good biocompatibility and high mechanical properties, and has become a common oral implant material.
[0003] At present, implants have become one of the important treatment methods in the fields of dentistry and orthopedics. However, there are still some problems with the current zirconia ceramic implants, such as poor bioactivity, insufficient tissue compatibility, and weak interface adhesion with surrounding tissues, which limit their application in the oral field. Among them, traditional implant materials include metal materials such as titanium alloys and stainless steel. Although they have high biocompatibility and biostability, they are prone to cause allergies and infections in some special cases.
[0004] Therefore, finding a better implant material has important clinical application value. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a nano-scale zirconia ceramic implant and a preparation method thereof, aiming to improve the bioactivity, tissue compatibility and interface adhesion of the zirconia ceramic implant, further promote its application in the oral field, and solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions: In a first aspect, the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixing connector, wherein the substrate is made of a nano-scale zirconia ceramic material, the surface treatment layer is made of a mixture of nano-scale zirconia ceramic and an organic polymer material, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate for fixing the implant in bone tissue.
[0007] The matrix of the nano-scale zirconia ceramic implant of the present invention is the main part, which is made of nano-scale zirconia material and has the advantages of high strength, high hardness, corrosion resistance and the like. A surface treatment layer is added when the main part is surface treated, which can enhance the bonding force between the implant and the bone tissue. In addition, by coating a coating containing bioactive molecules on the surface treatment layer, the bioactive molecule layer can better stimulate the proliferation of bone tissue. Finally, the implant is fixed in the bone tissue by a fixed connector to ensure function and stability.
[0008] As a further solution of the present invention, the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the particle diameter of the zirconia powder is between 30 and 80 nanometers.
[0009] As a further embodiment of the present invention, the stabilizer is any one of polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), sodium dodecyl benzene sulfonate (SDBS), sodium dodecyl sulfate, and polyvinyl pyrrolidone.
[0010] As a further solution of the present invention, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 30 to 80 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0011] As a further embodiment of the present invention, in step (1), the preparation of zirconium oxide powder comprises the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing the mixture thoroughly; (b) placing the stirred mixed solution in a heater and heating it to 100° C. to 200° C. to gradually dry the mixed solution to form a gel; (c) breaking the gel into small pieces and calcining the pieces in a tube furnace at a temperature between 500° C. and 800° C. for a time between 1 hour and 5 hours; (d) taking out the calcined sample from the furnace, and crushing and sieving it to obtain the nano-scale zirconium oxide powder.
[0012] As a further embodiment of the present invention, the organic solvent is ethanol or ethyl acetate solution, the mass fraction of the additive is 0.5% to 10%, the calcination temperature of the tube furnace is 600° C. to 700° C., and the calcination time is 2 hours to 4 hours.
[0013] As a further embodiment of the present invention, the average particle size of the nano-scale zirconium oxide powder is between 30 and 80 nanometers, the surface area is between 10 and 50 square meters per gram, and the crystal form of the nano-scale zirconium oxide powder is monoclinic or cubic.
[0014] As a further embodiment of the present invention, the additive is ammonium nitrate, ammonium sulfate, ethylene glycol, propylene glycol or polyvinyl alcohol.
[0015] As a further embodiment of the present invention, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the method comprises: 0.5-3wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 10-30 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 10-30 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0016] As a further solution of the present invention, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 100 to 200 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0017] As a further embodiment of the present invention, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0018] As a further embodiment of the present invention, the average particle size of the zirconium oxide powder is less than 100 nanometers, and the specific surface area is between 10 and 50 square meters per gram.
[0019] In a second aspect, the present invention further provides a method for preparing the nano-scale zirconia ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0020] Compared with the prior art, the nano-scale zirconia ceramic implant and the preparation method thereof of the present invention have the following beneficial effects: 1. High biocompatibility: Nano-scale zirconia ceramics have good biocompatibility, which can effectively reduce the rejection reaction between implants and human tissues and reduce the occurrence of complications.
[0021] 2. High mechanical strength: Nano-scale zirconia ceramics have very high mechanical strength and can withstand greater pressure and tension, which helps the implant to remain stable and firm in the mouth for a long time.
[0022] 3. Good biological activity: Nano-scale zirconia ceramics can promote the growth and differentiation of bone cells, help accelerate the regeneration and healing of bone tissue around the implant, and shorten the recovery time after implantation.
[0023] 4. Good wear resistance: Nano-level zirconia ceramics have very high wear resistance, which can effectively reduce the wear and corrosion of the implant surface and extend the service life of the implant.
[0024] 5. Good stability: Nano-level zirconia ceramics can effectively resist corrosion and oxidation, and have very high stability, which can ensure the long-term stability and safety of the implant in the oral cavity.
[0025] Therefore, the use of nano-sized zirconia ceramics to prepare implants can improve the biocompatibility, mechanical strength, bioactivity, wear resistance and stability of implants, which helps to improve the success rate of implants and the treatment effect of patients. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0027] Example 1 The embodiment of the present invention provides a nano-scale zirconia ceramic implant, wherein the matrix of the nano-scale zirconia ceramic implant is made by mixing zirconia powder and a PVP stabilizer, wherein the particle diameter of the zirconia powder is 60 nanometers.
[0028] The preparation method of the nano-scale zirconium oxide ceramic implant comprises the following steps: (1) The zirconium oxide particles are subjected to high-energy ball milling to reduce their diameter to a size of 60 nanometers and obtain a uniform particle distribution to obtain zirconium oxide powder.
[0029] (2) Mix nano-scale zirconium oxide powder and PVP stabilizer, add an appropriate amount of ethanol solvent, form a compressible mass, and use a pre-press to press out a green body.
[0030] (3) Sintering the green billet, using high temperature to cause strong interaction between its particles, thereby forming a dense zirconia ceramic body.
[0031] (4) Obtain the sintered zirconia ceramic body and perform fine processing through mechanical cutting and grinding to produce the final implant body.
[0032] (5) A coating containing bioactive molecules is applied to the surface treatment layer of the main part of the implant, and the implant is fixed in the bone tissue by a fixing connector.
[0033] Embodiment 2: The embodiment of the present invention provides a nano-scale zirconia ceramic implant, wherein the matrix of the nano-scale zirconia ceramic implant is prepared by mixing zirconia powder and SDBS stabilizer, wherein the particle diameter of the zirconia powder is 50 nanometers.
[0034] The preparation method of the nano-scale zirconium oxide ceramic implant comprises the following steps: (1) The zirconium oxide particles are subjected to high-energy ball milling to reduce their diameter to a size of 50 nanometers and obtain a uniform particle distribution to obtain zirconium oxide powder.
[0035] (2) Nano-scale zirconium oxide powder and SDBS stabilizer are mixed, and an appropriate amount of ethanol solvent is added to form a compressible mass, which is then pressed into a green body using a cold press.
[0036] (3) Sintering the green billet, using high temperature to cause strong interaction between its particles, thereby forming a dense zirconia ceramic body.
[0037] (4) Obtain the sintered zirconia ceramic body and perform fine processing through mechanical cutting and grinding to produce the final implant body.
[0038] (5) A coating containing bioactive molecules is applied to the surface treatment layer of the main part of the implant, and the implant is fixed in the bone tissue by a fixing connector.
[0039] Example 3 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 30 nanometers, and the stabilizer is polyvinyl pyrrolidone (PVP).
[0040] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 30 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0041] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is ethanol, the additive is ammonium nitrate, and the mass fraction of the additive is 0.5%; (b) placing the stirred mixed solution in a heater and heating it to 100° C. to gradually dry it to form a gel; (c) breaking the gel into small pieces and calcining them in a tube furnace at a temperature of 500° C. for 5 hours; (d) taking out the calcined sample from the furnace, crushing and sieving it to obtain the nano-scale zirconia powder, the average particle size of the nano-scale zirconia powder is 30 nanometers, the surface area is 10 square meters / gram, and the crystal form of the nano-scale zirconia powder is monoclinic.
[0042] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 0.5wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 30 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 30 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0043] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 100 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0044] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0045] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0046] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0047] Example 4 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 35 nanometers, and the stabilizer is polyethylene glycol (PEG).
[0048] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 35 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0049] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is an ethyl acetate solution, and the additive is ammonium sulfate, and the mass fraction of the additive is 1.5%; (b) placing the stirred mixed solution in a heater and heating it to 100° C. to 200° C. to gradually dry the mixed solution to form a gel; (c) breaking the gel into small pieces and calcining them in a tube furnace at 550°C for 4 hours; (d) taking out the calcined sample from the furnace, crushing and sieving it to obtain the nano-scale zirconia powder. The average particle size of the nano-scale zirconia powder is 35 nanometers, the surface area is 15 square meters / gram, and the crystal form of the nano-scale zirconia powder is monoclinic.
[0050] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 1wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 25 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 25 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0051] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 115 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0052] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0053] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0054] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0055] Example 5 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 45 nanometers, and the stabilizer is sodium dodecylbenzene sulfonate.
[0056] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 45 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0057] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is ethanol, the additive is ethylene glycol, and the mass fraction of the additive is 2%; (b) placing the stirred mixed solution into a heater and heating it to 125° C. to gradually dry the mixed solution to form a gel; (c) breaking the gel into small pieces and calcining them in a tube furnace at 650°C for 3.5 hours; (d) taking out the calcined sample from the furnace, crushing and sieving it to obtain the nano-scale zirconia powder, the average particle size of the nano-scale zirconia powder is 45 nanometers, the surface area is 25 square meters / gram, and the crystal form of the nano-scale zirconia powder is monoclinic.
[0058] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 2 wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 20 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 20 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0059] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 150 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0060] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0061] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0062] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0063] Example 6 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 50 nanometers, and the stabilizer is sodium dodecyl sulfate.
[0064] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 55 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0065] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is an ethyl acetate solution, the additive is propylene glycol, and the mass fraction of the additive is 4.5%; (b) placing the stirred mixed solution into a heater and heating it to 150° C. to gradually dry the mixed solution to form a gel; (c) breaking the gel into small pieces and calcining them in a tube furnace at 650°C for 3.5 hours; (d) taking out the calcined sample from the furnace, crushing and sieving it to obtain the nano-scale zirconia powder, the average particle size of the nano-scale zirconia powder is 50 nanometers, the surface area is 35 square meters / gram, and the crystal form of the nano-scale zirconia powder is monoclinic.
[0066] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 2.5wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 15 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 15 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0067] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 150 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0068] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0069] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0070] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0071] Example 7 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 70 nanometers, and the stabilizer is polyvinyl pyrrolidone.
[0072] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 75 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0073] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is an ethyl acetate solution, the additive is polyvinyl alcohol, and the mass fraction of the additive is 9%; (b) placing the stirred mixed solution into a heater and heating it to 180° C. to gradually dry the mixed solution to form a gel; (c) breaking the gel into small pieces and calcining them in a tube furnace at 550°C for 4.5 hours; (d) The calcined sample is taken out from the furnace, and is crushed and sieved to obtain the nano-scale zirconia powder. The nano-scale zirconia powder has an average particle size of 70 nanometers and a surface area of 35 square meters per gram. The crystal form of the nano-scale zirconia powder is cubic.
[0074] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 3wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 30 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 30 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0075] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 100 to 200 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0076] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0077] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0078] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0079] Example 8 An embodiment of the present invention provides a nano-scale zirconia ceramic implant, comprising a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector, wherein the substrate is made of a nano-scale zirconia ceramic material, wherein the nano-scale zirconia ceramic material is composed of nano-scale zirconia powder (ZrO2) and a stabilizer, wherein the zirconia powder has a particle diameter of 80 nanometers, and the stabilizer is polyvinyl pyrrolidone.
[0080] Wherein, the substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: (1) Preparation of zirconium oxide powder: high-energy ball milling of zirconium oxide particles to make the diameter of the zirconium oxide particles reach 80 nanometers and obtain uniform particle distribution to obtain zirconium oxide powder; (2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; (3) Green body sintering: The green body is sintered, and high temperature is used to cause strong interaction between the green body particles, thereby forming a dense zirconia ceramic body; (4) Implant processing: The sintered zirconia ceramic body is obtained and fine-processed by mechanical cutting and grinding to make the final implant body.
[0081] In this embodiment, in step (1), the preparation of zirconium oxide powder includes the following steps: (a) adding a zirconium oxide precursor and an additive into an organic solvent and stirring and mixing them thoroughly, wherein the organic solvent is ethanol, the additive is polyvinyl alcohol, and the mass fraction of the additive is 10%; (b) placing the stirred mixed solution in a heater and heating it to 100° C. to gradually dry it to form a gel; (c) breaking the gel into small pieces and placing them in a tube furnace for calcination at a temperature of 800° C. for 1 hour; (d) taking out the calcined sample from the furnace, crushing and sieving it to obtain the nano-scale zirconia powder. The average particle size of the nano-scale zirconia powder is 80 nanometers, the surface area is 50 square meters / gram, and the crystal form of the nano-scale zirconia powder is cubic.
[0082] In this embodiment, in step (2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the process includes: 3wt% of a stabilizer is mixed with zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder to prevent agglomeration and increase dispersibility. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 10 minutes to allow it to be completely adsorbed on the surface of the zirconium oxide powder. Before the stabilizer is added to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, which helps to speed up mixing and dispersion. When the stabilizer is added to the mixture, the mixing time is 10 minutes under the efficient stirring of the mixer, and ultrasonic-assisted stirring is used to further improve uniformity.
[0083] In this embodiment, when a green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 200 MPa in an argon atmosphere and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
[0084] The surface treatment layer is made of a mixture of nano-scale zirconium oxide ceramics and organic polymer materials, the bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, and the fixing connector is arranged at the root of the substrate to fix the implant in the bone tissue.
[0085] In this embodiment, the bioactive molecule layer is a coating containing proteins, enzymes and vitamins coated on the surface treatment layer.
[0086] The present invention also provides a method for preparing the nano-scale zirconium oxide ceramic implant, the steps of which are as follows: Step 1: preparing nano-scale zirconia ceramics: adding zirconia powder into an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2: Prepare the implant base: process the medical titanium alloy material into the shape of the implant; Step 3: Assembling the prepared nano-scale zirconia ceramics on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and evenly covering the surface of the implant base through coating and drying steps; Step 4: Calcination: Place the implant base coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant base to form a solid ceramic surface; Step 5: Surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6: Soaking and sterilizing: Soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.
[0087] In summary, the present invention provides a nano-scale zirconia ceramic implant, which includes a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector. The substrate is made of nano-scale zirconia ceramic material, which has the advantages of high strength, high hardness, corrosion resistance and the like. The surface treatment layer is made of a mixture of nano-scale zirconia ceramic and organic polymer material, which enhances the bonding force between the implant and the bone tissue. The bioactive molecule layer is a coating containing bioactive molecules coated on the surface treatment layer, which can stimulate the proliferation of bone tissue. The fixed connector is arranged at the root of the substrate to fix the implant in the bone tissue. The preparation method of the present invention includes the steps of preparing zirconia powder, zirconia ceramics, and implant processing. Among them, the steps of preparing zirconia powder include adding zirconia precursor and additives to an organic solvent, heating and drying to form a gel, breaking into small pieces, and placing in a tubular furnace for calcination treatment.
[0088] The advantages of the present invention are: the implant material is nano-scale zirconium oxide ceramics, which has excellent physical and chemical properties; the surface treatment layer can enhance the bonding force between the implant and the bone tissue; the bioactive molecule layer can stimulate the proliferation of bone tissue; the fixed connector can firmly fix the implant in the bone tissue to ensure its function and stability. In addition, the preparation method of the present invention is simple, low-cost, and can be mass-produced, and has good application prospects.
[0089] It should be noted that the nano-zirconia ceramic implant of the present invention is suitable for oral implantation, orthopedic implantation, etc. When using it, the appropriate implant model should be selected according to the specific conditions of the patient, and the implantation operation should be performed under the guidance of a professional doctor.
[0090] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A nano-scale zirconium oxide ceramic implant, It is characterized in that It includes a substrate, a surface treatment layer, a bioactive molecule layer and a fixed connector; wherein the substrate is made of nano-scale zirconia ceramic material, the surface treatment layer is made of a mixture of nano-scale zirconia ceramic and organic polymer material, the bioactive molecule layer is a coating containing bioactive molecules, and the fixed connector is arranged at the root of the substrate to fix the implant in the bone tissue.
2. The nano-scale zirconia ceramic implant according to claim 1, It is characterized in that The nano-scale zirconia ceramic material is composed of nano-scale zirconia powder and a stabilizer, wherein the particle diameter of the zirconia powder is between 30 and 80 nanometers.
3. The nano-scale zirconia ceramic implant according to claim 1, It is characterized in that The stabilizer is any one of polyvinyl pyrrolidone, polyethylene glycol, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and polyvinyl pyrrolidone.
4. The nano-scale zirconia ceramic implant according to claim 1 or 2, It is characterized in that The substrate is made of nano-scale zirconium oxide ceramic material, and the preparation method comprises the following steps: 1) Preparation of zirconia powder: high-energy ball milling of zirconia particles to make the diameter of zirconia particles reach 30 to 80 nanometers and obtain uniform particle distribution to obtain zirconia powder; 2) Preparation of zirconia ceramics: Mix nano-scale zirconia powder with a stabilizer and add an appropriate amount of solvent to form a compressible mass, and use a cold press or pre-press to press out a green body to obtain a solid green body of the desired size and shape; 3) Green body sintering: sintering the green body to obtain a zirconia ceramic body; 4) Implant processing: Obtain the sintered zirconia ceramic body and perform fine processing through mechanical cutting and grinding to make the final implant body.
5. The nano-scale zirconia ceramic implant according to claim 4, It is characterized in that In step 1), the preparation of zirconium oxide powder includes the following steps: a) adding zirconium oxide precursor and additives into an organic solvent and stirring and mixing them thoroughly; b) placing the stirred mixed solution into a heater, heating it to 100° C. to 200° C., and gradually drying it to form a gel; c) breaking the gel into small pieces and placing them in a tube furnace for calcination at a temperature between 500° C. and 800° C. for a time of 1 hour to 5 hours; d) taking out the calcined sample from the furnace, and crushing and sieving it to obtain the nano-scale zirconium oxide powder.
6. The nano-scale zirconia ceramic implant according to claim 5, It is characterized in that The organic solvent is ethanol or ethyl acetate solution, the mass fraction of the additive is 0.5% to 10%, the calcination temperature of the tube furnace is 600° C. to 700° C., and the calcination time is 2 hours to 4 hours.
7. The nano-scale zirconia ceramic implant according to claim 5, It is characterized in that The average particle size of the nano-scale zirconium oxide powder is between 30 and 80 nanometers, the surface area is between 10 and 50 square meters per gram, and the crystal form of the nano-scale zirconium oxide powder is monoclinic or cubic.
8. The nano-scale zirconia ceramic implant according to claim 5, It is characterized in that The additive is ammonium nitrate, ammonium sulfate, ethylene glycol, propylene glycol or polyvinyl alcohol.
9. The nano-scale zirconia ceramic implant according to claim 5, It is characterized in that In step 2), when the nano-scale zirconium oxide powder is mixed with the stabilizer, the following steps are included: 0.5-3wt% of the stabilizer is mixed with the zirconium oxide powder in a mass ratio of 1:5.5, and the stabilizer is coated on the surface of the zirconium oxide powder. After the stabilizer is fully mixed, it is allowed to stand at room temperature for 10-30 minutes until it is completely adsorbed on the surface of the zirconium oxide powder; Wherein, before adding the stabilizer to the zirconium oxide powder, the zirconium oxide powder is preliminarily mixed by a ball mill, and when the stabilizer is added to the mixture, the mixing time is 10-30 minutes under the efficient stirring of the stirrer, and ultrasonic assisted stirring is used; When the green body is pressed out using a cold press or a pre-press, it is pressed at an isostatic pressure of about 100 to 200 MPa in an argon atmosphere, and then left to solidify for 2 hours to obtain a solid green body of the desired size and shape.
10. A method for preparing a nano-scale zirconia ceramic implant according to any one of claims 1 to 9, It is characterized in that Here are the steps: Step 1, preparing nano-scale zirconia ceramics: adding zirconia powder to an organic solution, and preparing nano-scale zirconia ceramics after mechanical mixing, drying, and calcining; Step 2, preparing the implant base: processing the medical titanium alloy material into the shape of the implant; Step 3, assembling the prepared nano-scale zirconia ceramic on the surface of the implant base: adding nano-scale zirconia ceramic powder to the organic solution, and uniformly covering the surface of the implant base through coating and drying steps; Step 4, calcination: placing the implant substrate coated with nano-scale zirconia ceramics into a sintering furnace for high-temperature calcination to combine the zirconia ceramics with the implant substrate to form a solid ceramic surface; Step 5, surface treatment: The surface of the nano-scale zirconia ceramic is treated by pickling and polishing to obtain a smooth surface and appropriate surface roughness; Step 6, soaking and sterilization: soak the prepared implant in a biological fluid of physiological saline to remove residual substances and impurities on the surface, and sterilize the implant to ensure its sterility to avoid infection and other problems; Step 7: Packaging: The prepared implants are packaged to ensure their quality and hygiene during transportation and storage.