Silicon modified alumina catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde

Through the preparation of silicon-modified alumina catalysts, Si-O-Al bonds and cesium active centers are used to improve the selectivity and reactivity of methyl acrylate, solving the problems of insufficient selectivity and stability of existing catalysts and achieving efficient Aldol condensation reaction of methyl acetate and formaldehyde.

CN118751231APending Publication Date: 2024-10-11UNIV OF CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410926249.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing alumina and silica catalysts have problems with insufficient selectivity and stability in the aldol condensation reaction of methyl acetate and formaldehyde. The alumina catalyst has low selectivity and short single-pass life, and the silica catalyst has poor thermal stability. And the activity decreases.

Method used

Through the preparation method of silicon-modified alumina catalyst, the organic silicon source is combined with the alumina carrier using liquid deposition method and impregnation method to form Si-O-Al bond, and cesium is introduced to form the silicon-oxycesium active center to improve the catalyst's performance Selectivity and reactivity.

Benefits of technology

It improves the selectivity of methyl acrylate and the single-pass life of the catalyst, while maintaining the long-term stability of alumina, reducing energy consumption and separation difficulty, and has important industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751231A_ABST
    Figure CN118751231A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a catalyst for synthesizing methyl acrylate. The catalyst mainly comprises two parts, one part is silicon modified aluminum oxide, and the other part is cesium oxide with surface alkalinity. The loading amount of the active component accounts for 1-15 wt% of the total mass of the catalyst; and the silicon dioxide modifier accounts for 1-15 wt% of the total mass of the catalyst. Aluminum oxide contains strong acid sites and has low selectivity on methyl acrylate, and carbon deposition is easily generated in the reaction process, so that the one-way service life of the catalyst is relatively short. Inert silicon dioxide is deposited on the surface of aluminum oxide, so that strong acid sites on the surface of the aluminum oxide are greatly reduced, and cesium is introduced to form a silicon-oxygen-cesium active center, so that the activity and stability of the catalyst are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts for synthesizing methyl acrylate through aldol condensation of methyl acetate and formaldehyde, and particularly relates to preparation and application of a silicon-modified alumina catalyst. Background Art

[0002] Methyl acrylate is an important organic raw material and synthetic resin monomer. It has a wide range of downstream uses, mainly in adhesives, coatings, super absorbent resins (SPA) and other fields. The industrial production methods of acrylic acid and its esters mainly include cyanohydrin method, acetylene carbonylation method, ethylene method and propylene oxidation method. Due to the problems of equipment corrosion, high raw material toxicity, harsh operating conditions, and dependence on oil and natural gas energy in these methods, in recent years, the method of preparing methyl acrylate by one-step aldol condensation reaction using formaldehyde and methyl acetate as raw materials has attracted widespread attention. The aldol condensation reaction of methyl acetate and formaldehyde is a typical acid-base catalytic reaction. In the existing catalyst development process, two carriers are mainly involved: one is alumina; the other is silica. The catalyst with alumina as the carrier has a higher conversion rate of methyl acetate, a long long-term life, but a lower selectivity and a short one-way life; while the catalyst with silica as the carrier has a higher selectivity for methyl acrylate, a long one-way life, but a lower conversion rate and poor long-term experimental stability. Due to the poor thermal stability of silica, the pore structure is easily destroyed in long-term experiments, and the specific surface area decreases seriously, causing the activity of the catalyst to continue to decline during long-term operation. Alumina has high thermal stability and its pore structure is not easily destroyed during long-term operation, but the selectivity of the catalyst for methyl acrylate is low, which increases the difficulty of separation, and the catalyst has a short single-pass life, which increases the energy consumption of the operation process. It can be seen that the development of an efficient and stable catalyst has important practical significance. Silanization by chemical vapor deposition (CVD) or chemical liquid deposition (CLD) is an effective method to remove acid sites on the surface of the carrier. During the silanization process, the modifier (organic silicon compound with a large molecular weight, such as tetraethyl orthosilicate (TEOS) or methyl silicone oil) is deposited on the surface of alumina, interacts with Al-OH and Al-O-, forms Si-O-Al bonds, and finally decomposes into silica after calcination in air. The inert silica is deposited on the surface of alumina, which greatly reduces the strong acid sites on the surface of alumina, and then cesium is introduced to form silane-cesium active centers, further improving the reaction activity of the catalyst. This not only improves the selectivity and single-pass life of the catalyst, but also improves the reaction activity of the catalyst. The use of silicon-modified alumina as a carrier to load cesium acid-base bifunctional catalyst in the aldol condensation reaction of methyl acetate and formaldehyde has very important practical significance and industrial application value. Summary of the invention

[0003] The present invention provides a silicon-modified alumina catalyst for use in the synthesis of methyl acrylate from methyl acetate and formaldehyde. The catalyst obtained by the present invention can improve the stability of aldol condensation and the selectivity of methyl acrylate. The purpose of the present invention is achieved by adopting the following technical scheme: A method for preparing a silicon-modified alumina catalyst for the synthesis of methyl acrylate from methyl acetate and formaldehyde, comprising the following steps: 1) Modification of alumina carrier: Prepare a silicon-containing deposition liquid according to the mass ratio, put alumina into the deposition liquid by liquid phase deposition method, and obtain a silicon-modified alumina carrier for loading active components after deposition, rotary evaporation, drying and calcination; 2) Active component loading: a salt solution containing active components is prepared according to a mass ratio, and the prepared solution is mixed with a modified carrier by an equal volume impregnation method. After impregnation adsorption, drying and calcination, a silicon-modified alumina catalyst loaded with active components is obtained; Furthermore, the silicon-containing deposition liquid in step 1) is an organic solution containing different organic silicon sources. The organic silicon sources include methyl orthosilicate, ethyl orthosilicate, dimethylsilane, and 3-chloropropyltrimethoxysilane; the organic solvents include strongly polar DMF (dimethylformamide), medium polar ethanol, and non-polar cyclohexane. The deposition temperature is 20-80°C, the deposition stirring rate is 400 rpm, and the deposition time is 2-16h; the rotary evaporation temperature is 60-100°C; the drying temperature is 80-120°C, and the drying time is 2-4h; the calcination temperature is 400-700°C, and the calcination time is 2-8h; Furthermore, the salt solution of the active component in step 2) is an aqueous solution or alcohol solution of one or more of cesium nitrate, cesium acetate, cesium carbonate, and cesium formate; the impregnation adsorption time is 6-20 hours; the drying temperature is 80-120°C, the drying time is 2-4 hours; the roasting temperature is 400-700°C, and the roasting time is 2-8 hours; A silicon-modified alumina catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde is prepared by the above-mentioned preparation method. In the preparation method of a silicon-modified alumina catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde, the mass ratio of silicon-modified auxiliary agent to active component and carrier alumina is 0.01-0.14; 0.02-0.25. The aldol condensation reaction of methyl acetate and formaldehyde is a typical acid-base catalytic reaction. The efficient active reaction center is a medium-strong acid-base site. The strong acid site contained in alumina itself will reduce the selectivity of the reaction to methyl acrylate, and it is easy to produce carbon deposition, which makes the catalyst single-pass life shorter and the deactivation rate faster. Inert silicon dioxide is deposited on the surface of alumina, so that the strong acid sites on the surface of alumina are greatly reduced, and cesium is introduced to form a cesium-silicon active center, which further improves the reaction activity of the catalyst. This not only improves the catalyst selectivity and single-pass life, but also improves the reaction activity of the catalyst. Compared with the existing catalysts, the advantages of the present invention are: the catalyst prepared by the method provided by the present invention has an improved yield of methyl acrylate and a longer single-pass life while retaining the long-term stability of alumina, and has certain industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 This is the relationship between the yield of methyl acrylate and the reaction time of Cat8 and Cat9 catalysts. DETAILED DESCRIPTION

[0004] The present invention is further described in detail below in conjunction with specific implementation examples, but it should not be understood that the subject scope of the present invention is limited to the following implementation examples. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to common technical knowledge and customary means in the field, which should be included in the scope of the present invention: Example 1

[0005] 1. Dissolve 2 ml of tetraethyl orthosilicate in 100 ml of cyclohexane, mix 10 g of alumina with the above solution and deposit at 40 ° C for 4 hours, then remove the solvent cyclohexane by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 1.372g of cesium nitrate and add 8.6ml of deionized water to dissolve it into an aqueous solution, weigh 10g of the modified carrier and add it into the impregnation solution, soak and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat1; Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 2

[0006] 1. Dissolve 2 ml of dimethylsilane in 100 ml of ethanol, mix 10 g of alumina with the above solution and deposit at 40 ° C for 4 hours, then remove the solvent ethanol by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 0.686g of cesium nitrate and add it to 8.6ml of deionized water to dissolve it into an aqueous solution. Weigh 10g of the modified carrier and add it to the impregnation solution. Impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat2. Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 3

[0007] 1. Dissolve 2 ml of 3-chloropropyltrimethoxysilane in 100 ml of ethanol, mix 10 g of alumina with the above solution and deposit at 60 ° C for 1 hour, then remove the solvent ethanol by rotary evaporation at 60 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 700 ° C for 2 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 0.343g of cesium nitrate and add it to 8.6ml of deionized water to dissolve it into an aqueous solution. Weigh 10g of the modified carrier and add it to the impregnation solution. Impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat3. Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 4

[0008] 1. Dissolve 2 ml of ethyl orthosilicate in 100 ml of ethanol, mix 10 g of alumina with the above solution and deposit at 80 ° C for 10 hours, then remove the solvent ethanol by rotary evaporation at 60 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 400 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 0.686g of cesium nitrate and add it to 8.6ml of deionized water to dissolve it into an aqueous solution. Weigh 10g of the modified carrier and add it to the impregnation solution. Impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat4. Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 5

[0009] 1. Dissolve 2 ml of ethyl orthosilicate in 100 ml of dimethylformamide, mix 10 g of alumina with the above solution and deposit at 100 ° C for 4 hours, then remove the solvent dimethylformamide by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 0.137g of cesium nitrate and add it to 8.6ml of deionized water to dissolve it into an aqueous solution. Weigh 10g of the modified carrier and add it to the impregnation solution. Adsorb it for 12h, dry it at 110℃ for 4h, and finally calcine it at 600℃ for 2h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat5. Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 6

[0010] 1. Dissolve 2 ml of tetraethyl orthosilicate in 100 ml of cyclohexane, mix 10 g of alumina with the above solution and deposit at 40 ° C for 4 hours, then remove the solvent cyclohexane by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 2.058g of cesium nitrate and add it to 8.6ml of deionized water to dissolve it into an aqueous solution. Weigh 10g of the modified carrier and add it to the impregnation solution. Adsorb it for 12h, dry it at 110℃ for 4h, and finally calcine it at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat6. Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 7

[0011] 1. Dissolve 8 ml of tetraethyl orthosilicate in 100 ml of cyclohexane, mix 10 g of alumina with the above solution and deposit at 40 ° C for 4 hours, then remove the solvent cyclohexane by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 1.372g of cesium nitrate and add 8.6ml of deionized water to dissolve it into an aqueous solution, weigh 10g of the above modified carrier and add it into the above impregnation solution, impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 400℃ for 6h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat7; Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Example 8

[0012] 1. Dissolve 12 ml of tetraethyl orthosilicate in 100 ml of cyclohexane, mix 10 g of alumina with the above solution and deposit at 40 ° C for 4 hours, then remove the solvent cyclohexane by rotary evaporation at 80 ° C, then dry at 110 ° C for 2 hours, and finally calcine at 600 ° C for 6 hours to obtain the silicon-modified carrier Si-Al2O3; 2. Weigh 1.372g of cesium nitrate and add 8.6ml of deionized water to dissolve it into an aqueous solution, weigh 10g of the above modified carrier and add it into the above impregnation solution, impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Si-Al2O3 loaded with active components and record it as Cat8; Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Comparative Example 1

[0013] Weigh 1.372g of cesium nitrate and add it into 8.6ml of deionized water to dissolve it into an aqueous solution, weigh 10g of aluminum oxide and add it into the above impregnation solution, impregnate and adsorb for 12h, dry at 110℃ for 4h, and finally calcine at 500℃ for 4h to obtain the catalyst Cs / Al2O3 loaded with active components and record it as Cat9; Catalyst test: The performance evaluation of the catalyst was carried out in a fixed bed reactor. The inner diameter of the reaction tube was 10 mm, the catalyst loading was 4 g, the feed flow rate was 0.06 ml / min, and the feedstock contained methyl acetate, formaldehyde, and methanol, and their molar ratio was 1 / 2 / 1. The reactor temperature was 360 ° C and operated at normal pressure. After 3 hours of stable operation, the liquid products and tail gas were sampled and analyzed every 2 hours. The experimental repeatability and stability were good, and the quality difference before and after the reaction was within 4%. The liquid products were analyzed by FID gas chromatography, and the gas products were analyzed by TCD gas chromatography. The evaluation results are shown in Table 1 Table 1: Catalyst No. Methyl acetate conversion rate / % Methyl acrylate selectivity / % Cat 1 28.9 27.8 Cat 2 16.2 21.5 Cat 3 10.2 20.2 Cat 4 15.2 23.3 Cat 5 17.2 20.1 Cat 6 40.2 25.6 Cat 7 27.8 43.7 Cat 8 28.9 71.2 Cat 9 35.2 22.1

Claims

1. A silicon-modified alumina catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde, characterized in that: The catalyst carrier is alumina modified by silicon dioxide, and the active component is cesium.

2. The catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde according to claim 1, characterized in that: The loading amount of the active component accounts for 1-15wt% of the total mass of the catalyst; the loading amount of the silicon dioxide modifier accounts for 1-15wt% of the total mass of the catalyst.

3. The catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde according to claim 1, characterized in that The preparation method of the catalyst comprises the following steps: (1) Calcinate alumina at 600°C for 3-6 hours; (2) placing the alumina carrier obtained in (1) into a deposition liquid, wherein the deposition liquid is a silicon-containing organic solution, and performing liquid phase deposition at 20-80° C., with a deposition stirring rate of 100-400 rpm and a deposition time of 2-16 h; After the deposition is completed, the mixture is subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature is 60-100°C, and the rotary evaporation time is 0.5h; finally, the mixture is dried, the drying temperature is 80-120°C, and the drying time is 2-4h; (3) calcining the solid obtained in (2) at 400-700° C. for 2-8 h to obtain a silicon-modified alumina carrier; (4) The silicon-modified alumina carrier obtained in (3) is loaded with active components by using an equal volume impregnation method to mix the prepared cesium-containing salt solution with the silicon-modified alumina carrier. After impregnation, adsorption, drying and calcination, a silicon-modified alumina catalyst loaded with active components is obtained.

4. The method for preparing a catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde according to claim 3, characterized in that: The cesium salt solution is an aqueous solution or alcohol solution of one or more of cesium nitrate, cesium acetate, cesium carbonate, and cesium formate; the impregnation adsorption time is 6-20 hours; the drying temperature is 80-120° C., and the drying time is 2-4 hours; the roasting temperature is 400-700° C., and the roasting time is 2-8 hours.