Metal monatomic doped carbon nanomaterial catalyst as well as preparation method and application thereof

By dispersing M-N complexes in graphyne to form a metal single atom doped nanocarbon material catalyst, the problems of short catalyst life and high potential in the oxygen reduction reaction are solved, achieving efficient oxygen reduction activity and stability, and meeting the performance requirements There is a need for excellent and inexpensive non-platinum catalysts.

CN118751271AActive Publication Date: 2024-10-11SHANDONG UNIV

Patent Information

Application Number
CN202410810253.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-11
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing oxygen reduction catalysts have problems such as high reaction potential and short catalyst life in oxygen reduction reactions, especially the rarity and high cost of platinum-based materials. This has led to the search for non-platinum-based catalysts with excellent performance and low price becoming a research hotspot. .

Method used

By first forming an M-N bonded complex with a nitrogen-containing ligand and a metal salt, and dispersing it in graphyne, a metal single-atom doped nanocarbon material catalyst is formed through high-temperature annealing to improve the ratio of M-N active sites and the electronic structure of the catalyst. Control and control to obtain a graphyne-based oxygen reduction catalyst with excellent performance.

Benefits of technology

Atomic-level dispersion of metal atoms is achieved, catalytic activity and stability are improved, catalyst life is extended, and excellent oxygen reduction activity and toxicity resistance are shown in applications such as zinc-air fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751271A_ABST
    Figure CN118751271A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oxygen reduction catalysts, in particular to a metal monatomic doped carbon nanomaterial catalyst as well as a preparation method and application thereof. According to the preparation method, the nitrogen-containing ligand and the metal salt are coordinated to form the M-N bonded complex, so that the proportion of effective M-N active sites can be increased, and then the graphdiyne and the M-N complex are mixed to limit the complex in molecular pores, so that metal atoms are subjected to atomic-scale dispersion, and the metal atoms are dispersed at the same time. Therefore, the monatomic doped graphdiynyl oxygen reduction catalyst material is finally obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of oxygen reduction catalysts, and in particular to a metal single atom doped nano-carbon material catalyst and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] At present, fossil energy, led by coal, oil and natural gas, is still the main energy consumed by humans, and the shortage of fossil energy and the global warming and climate change caused by the use of fossil energy are also attracting widespread attention. Therefore, the research and development of sustainable clean energy storage and conversion technology has become the key to today's world. Converting chemical energy into electrical energy by electrochemical oxidation and reduction and storing it in the form of batteries is a more feasible and economical approach. Among them, high-capacity energy conversion systems, such as zinc-air batteries and fuel cells, have attracted widespread attention for their low or even zero emission characteristics and high efficiency. Among them, the oxygen reduction reaction (ORR) is an important cathode reaction in the fuel cell device and is also the key to the realization of the device. However, the shortcomings of too high reaction potential and too short catalyst life have always plagued the research on oxygen reduction reaction. At present, there are two main types of oxygen reduction catalysts, namely platinum group metal (PGM catalyst) and non-platinum group catalysts (mainly transition metals and nitrogen-doped carbon materials). However, platinum materials have the disadvantages of being rare, expensive, unstable, and susceptible to poisoning, which has accelerated the search for non-platinum catalysts. At present, common non-platinum catalysts include transition metal oxides, carbon-based materials, transition metal macrocyclic compounds, etc. Researching non-platinum catalysts with excellent performance and low price has become one of the main directions of oxygen reduction reaction research.

[0004] In recent years, single-atom catalysts, as an emerging field of heterogeneous catalysis, have attracted widespread attention due to their high atomic utilization and catalytic activity comparable to that of precious metal catalysts. Among them, the metal-nitrogen-carbon (MNC) structure uses nitrogen to anchor dispersed metal atoms to form single-atom sites, and this type of site often exhibits good catalytic activity. However, in general, MNC catalysts are mostly made by combining metal salts with carbon materials and then doping them with N atoms. In this case, the metal atoms are less coordinated with nitrogen, and the proportion of effective MN active sites is small, which will affect the final catalyst performance. Summary of the invention

[0005] In order to overcome the above problems, the present invention provides a metal single atom doped nano-carbon material catalyst and its preparation method and application. In the present invention, the nitrogen-containing ligand is first coordinated with the metal salt to form an MN bonding complex, which can increase the proportion of effective MN active sites, and then after graphyne is mixed with the MN complex, the complex can be confined in the molecular pore, so that the metal atoms are dispersed at the atomic level, and thus a single-atom doped graphyne-based oxygen reduction catalyst material is finally obtained.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing a metal single atom-doped nanocarbon material catalyst, comprising:

[0008] The nitrogen-containing ligand and the metal salt are added to the solvent A, and the reaction is stirred to form the complex MN; the nanocarbon material and the complex MN are dispersed in the solvent B, and the reaction is stirred for pre-adsorption; after the reaction is completed, the solvent B is removed to obtain a catalyst precursor; the catalyst precursor is first heated to 600-750° C. in an inert gas atmosphere, and then heated to 850-950° C. in a nitrogen atmosphere for calcination to obtain a metal single atom doped nanocarbon material catalyst;

[0009] Wherein, the nano carbon material is nano graphene (GDY) or nano hydrogen-substituted graphene (HsGDY).

[0010] The second aspect of the present invention provides a metal single atom doped nano-carbon material catalyst prepared by the above preparation method.

[0011] The third aspect of the present invention provides the use of the above-mentioned metal single atom doped nanocarbon material catalyst as an oxygen reduction working electrode catalyst or air electrode catalyst in a zinc-air fuel cell, a hydrogen-oxygen fuel cell, a magnesium-air fuel cell or an aluminum-air fuel cell.

[0012] The beneficial effects of the present invention are:

[0013] (1) The present invention first coordinates the nitrogen-containing ligand with the metal salt to form an MN bonding complex, which can increase the proportion of effective MN active sites. However, the MN complex is large in size and difficult to disperse in traditional carbon materials. Therefore, it is easy to agglomerate during high-temperature annealing, which is not conducive to the formation of high-density atomic-level active sites. Graphdiyne is rich in sp and sp 2 GDY is a two-dimensional carbon network allotrope. GDY itself has large and controllable molecular pores. After GDY is mixed with MN complex, the complex can be confined in the molecular pores, so that the metal atoms can be dispersed at the atomic level, thus finally obtaining a single-atom-doped GDY-based oxygen reduction catalyst material.

[0014] (2) The nitrogen-containing ligand is first coordinated with the metal salt to form an MN bonding complex, which can change the ratio of the central atom to the coordinated atom and conveniently adjust the number of coordinated atoms in the final reaction site, thereby regulating the electronic structure of the transition metal atoms in the catalyst product and obtaining an electrocatalyst material with excellent performance.

[0015] (3) Compared with the MNC catalyst formed by combining metal salts with carbon materials and then doping with N atoms, the MN active sites in the single-atom doped graphyne-based oxygen reduction catalyst material in the present invention are relatively high, and therefore have good catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0017] Figure 1 The SEM and TEM images of graphyne; a is the SEM image, and b is the TEM image;

[0018] Figure 2 The SEM and TEM images of the single-atom doped graphyne oxygen reduction catalyst Zn-N-GDY synthesized in Example 1; wherein a is a SEM image and b is a TEM image;

[0019] Figure 3 The oxygen reduction activity test results of the catalysts prepared in Example 1 and Comparative Examples 1-2 in Experimental Example 1;

[0020] Figure 4 The anti-toxicity test results of Zn-N-GDY prepared in Example 1;

[0021] Figure 5 ORR polarization curves of Zn-N-GDY prepared in Example 1 before and after 5000 CV cycles;

[0022] Figure 6 Where a is the LSV curve of Zn-N-GDY prepared in Example 1 at different rotation speeds, b is the yield of H2O2 during the catalytic process, and c is the corresponding electron transfer number during the catalytic process. DETAILED DESCRIPTION

[0023] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0024] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0025] A first typical embodiment of the present invention provides a method for preparing a metal single atom-doped nanocarbon material catalyst, comprising:

[0026] The nitrogen-containing ligand and the metal salt are added to the solvent A, and the reaction is stirred to form the complex MN; the nanocarbon material and the complex MN are dispersed in the solvent B, and the reaction is stirred for pre-adsorption; after the reaction is completed, the solvent B is removed to obtain a catalyst precursor; the catalyst precursor is first heated to 600-750° C. in an inert gas atmosphere, and then heated to 850-950° C. in a nitrogen atmosphere for calcination to obtain a metal single atom doped nanocarbon material catalyst;

[0027] Wherein, the nano-carbon material is nano-graphene (GDY) or nano-hydrogen-substituted graphene (HsGDY).

[0028] In one or more embodiments, the metal salt is preferably one of anhydrous ZnCl2, anhydrous FeCl3 or copper acetylacetonate.

[0029] In one or more embodiments, the nitrogen-containing ligand is preferably one of pyrazole-3-carboxylic acid, urea, cyanamide, dicyandiamide or 2,2-bipyridine.

[0030] In one or more embodiments, the molar ratio of the metal salt to the nitrogen-containing ligand is 1:1 to 1:100, preferably 1:10.

[0031] In one or more embodiments, the stirring reaction to form the complex MN takes 20 to 30 hours.

[0032] In one or more embodiments, solvent A is preferably ethanol or deionized water, and solvent B is preferably an ethanol solution with a volume concentration of 20% to 100%. The preferred ethanol solution is a mixed solution of ethanol and deionized water.

[0033] In one or more embodiments, the molar ratio of the metal salt to graphyne or hydrogen-substituted graphyne is 0.1% to 10%, preferably 1% to 2.5%.

[0034] In one or more embodiments, the stirring pre-adsorption time is 20 to 30 hours.

[0035] In one or more embodiments, the calcination time is 0.5 to 2 hours, preferably 0.5 hours.

[0036] In one or more embodiments, during calcination, the heating rate is 1 to 10° C. / min, more preferably 5° C. / min.

[0037] A second typical embodiment of the present invention provides a metal single atom-doped nanocarbon material catalyst prepared by the above preparation method.

[0038] A third typical embodiment of the present invention provides the use of the above-mentioned metal single atom doped nanocarbon material catalyst as an oxygen reduction working electrode catalyst or air electrode catalyst in a zinc-air fuel cell, a hydrogen-oxygen fuel cell, a magnesium-air fuel cell or an aluminum-air fuel cell.

[0039] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0040] Using copper foil as the substrate, graphyne and hydrogen-substituted graphyne were synthesized by cross-coupling reaction, and then peeled off from the copper foil to obtain powder samples. The morphology of the synthesized graphyne was characterized by scanning electron microscopy (SEM) and transmission microscopy (TEM). The results are as follows: Figure 1 Said, from Figure 1 It can be seen that the internal and external morphologies of GDY are both pore network structures.

[0041] Example 1

[0042] Take 2mg of anhydrous ZnCl2 and 4mg of cyanamide and dissolve them in 10mL of ethanol, stir for 24h to obtain Zn-N complex. Take 10mg of GDY and dissolve it in ethanol. After ultrasonic dispersion for 0.5h, add Zn-N complex, continue stirring for 24h, use 500mL of deionized water to filter, evaporate ethanol at 85℃ to obtain catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it and then pass argon gas, repeat three times to ensure that O2 is excluded. Heat to 650℃ in an argon atmosphere. At this time, stop passing argon gas and pass NH3 to exclude argon gas. Heat to 900℃ in an NH3 atmosphere, continue pyrolysis for 0.5h and then cool to room temperature to obtain a single-atom doped graphyne oxygen reduction catalyst Zn-N-GDY. The synthesized single-atom doped graphyne oxygen reduction catalyst Zn-N-GDY was characterized by scanning electron microscopy (SEM) and transmission microscopy (TEM), and the results are as follows Figure 2 Said, from Figure 2 It can be seen that the structure of GDY is maintained during high-temperature calcination.

[0043] Example 2

[0044] Take 2mg of anhydrous ZnCl2 and 2mg of 2,2-bipyridine and dissolve them in 10mL of ethanol. Stir for 24h to obtain Zn-N complex. Take 10mg of HsGDY and dissolve it in 50% ethanol by volume. After ultrasonic dispersion for 0.5h, add Zn-N complex and continue stirring for 24h. Use 500mL of deionized water to filter and evaporate ethanol at 85℃ to obtain catalyst precursor. Transfer the powder to a quartz boat and put it into a tubular heating furnace. After vacuuming with a vacuum pump, introduce argon and repeat three times to ensure that O2 is excluded. Heat to 650℃ in an argon atmosphere. At this time, stop passing argon and introduce NH3 to exclude argon. Heat to 900℃ in an NH3 atmosphere, continue pyrolysis for 0.5h and cool to room temperature to obtain a single-atom doped graphene oxygen reduction catalyst Zn-N-HsGDY.

[0045] Example 3

[0046] Take 1.5 mg of anhydrous FeCl3 and 2 mg of pyrazole-3-carboxylic acid and dissolve them in 10 mL of ethanol, stir for 24 hours to obtain Fe-N complex. Take 10 mg of GDY and dissolve it in ethanol. After ultrasonic dispersion for 0.5 hours, add Fe-N complex and continue stirring for 24 hours. Use 500 mL of deionized water to filter and evaporate ethanol at 85°C to obtain a catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it to vacuum, and then pass argon gas. Repeat three times to ensure that O2 is excluded. Heat to 600°C in an argon atmosphere. At this time, stop passing argon gas and pass NH3 to exclude argon gas. Heat to 850°C in an NH3 atmosphere, continue pyrolysis for 0.5 hours, and then cool to room temperature to obtain a single-atom doped graphene oxygen reduction catalyst Fe-N-GDY.

[0047] Example 4

[0048] Take 1.5 mg of anhydrous FeCl3 and 2 mg of dicyandiamide and dissolve them in 10 mL of ethanol, stir for 24 hours to obtain Fe-N complex. Take 10 mg of GDY and dissolve it in ethanol. After ultrasonic dispersion for 0.5 hours, add Fe-N complex, continue stirring for 24 hours, use 500 mL of deionized water to filter, evaporate ethanol at 85 ° C to obtain a catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it to vacuum, and then pass argon gas. Repeat three times to ensure that O2 is excluded. Heat to 750 ° C in an argon atmosphere. At this time, stop passing argon gas, pass NH3 to exclude argon gas. Heat to 950 ° C in an NH3 atmosphere, continue pyrolysis for 0.5 hours, and then cool to room temperature to obtain a single-atom doped graphene oxygen reduction catalyst Fe-N-GDY.

[0049] Example 5

[0050] Take 1.2 mg of copper acetylacetonate and 4 mg of 2,2-bipyridine and dissolve them in 10 mL of deionized water, stir for 24 hours to obtain a Cu-N complex. Take 10 mg of HsGDY and dissolve it in ethanol with a volume concentration of 80%. After ultrasonic dispersion for 0.5 hours, add the Cu-N complex, continue stirring for 24 hours, use 500 mL of deionized water to filter, evaporate the ethanol at 85 ° C to obtain a catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it to a vacuum, and then pass argon gas. Repeat three times to ensure that O2 is excluded. Heat to 750 ° C in an argon atmosphere. At this time, stop passing argon gas, pass NH3 to exclude argon gas. Heat to 900 ° C in an NH3 atmosphere, continue pyrolysis for 0.5 hours, and then cool to room temperature to obtain a single-atom doped graphene oxygen reduction catalyst Cu-N-HsGDY.

[0051] Example 6

[0052] Take 2mg of copper acetylacetonate and 4mg of urea and dissolve them in 10mL of deionized water, stir for 24h to obtain a Cu-N complex. Take 10mg of GDY and dissolve it in ethanol. After ultrasonic dispersion for 0.5h, add the Cu-N complex, continue stirring for 24h, use 500mL of deionized water to filter, evaporate the ethanol at 85℃ to obtain a catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it to vacuum, and then pass argon gas. Repeat three times to ensure that O2 is excluded. Heat to 750℃ in an argon atmosphere. At this time, stop passing argon gas, pass NH3 to exclude argon gas. Heat to 900℃ in an NH3 atmosphere, continue pyrolysis for 0.5h, and then cool to room temperature to obtain a single-atom doped graphene oxygen reduction catalyst Cu-N-GDY.

[0053] Comparative Example 1

[0054] Take 2mg of anhydrous ZnCl2 and 10mg of GDY and dissolve them in 10mL of ethanol respectively, stir for 24h to obtain Zn-GDY. Use 500mL of deionized water to filter, evaporate the ethanol at 85℃ to obtain a catalyst precursor. Transfer the catalyst precursor to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it to vacuum, and then pass argon gas, repeat three times to ensure that O2 is excluded. Heat to 650℃ in an argon atmosphere. At this time, stop passing argon gas, pass NH3 to exclude argon gas. Heat to 900℃ in an NH3 atmosphere, continue pyrolysis for 0.5h, and then cool to room temperature to obtain a single-atom doped graphyne oxygen reduction catalyst Zn-N0-GDY.

[0055] Comparative Example 2

[0056] Take 10 mg of GDY and transfer it to a quartz boat, put it into a tubular heating furnace, use a vacuum pump to evacuate it, and then pass argon gas. Repeat three times to ensure that O2 is excluded. Heat to 650°C in an argon atmosphere. At this time, stop passing argon gas, pass NH3 to exclude argon gas. Heat to 900°C in an NH3 atmosphere, continue pyrolysis for 0.5h, and then cool to room temperature to obtain nitrogen atom-doped graphene oxygen reduction catalyst N0-GDY.

[0057] Experimental Example 1

[0058] The oxygen reduction activity of the catalysts prepared in Example 1 and Comparative Examples 1-2 was tested in an electrolyte of 0.1 M KOH using a rotating disk electrode. The rotation speed was fixed at 1600 rpm and the loading was 0.4 mg cm -2 , the scanning speed is 5mV s -1 The polarization curve of the catalyst was obtained under the conditions of Figure 3 As shown, metal-free N-doped graphyne itself has extremely low oxygen reduction performance. The performance of transition metal directly adsorbed on graphyne without pre-coordination and then doped with N atoms is improved but still cannot reach the ideal catalytic performance. The single-atom Zn-N-GDY formed by pre-coordination of metal and ligand and then dispersion into graphyne has excellent oxygen reduction activity.

[0059] Experimental Example 2

[0060] The Zn-N-GDY prepared in Example 1 was tested for anti-toxicity. Figure 4 As shown. Figure 4 It can be seen that the LSV curve of Zn-N-GDY changes little before and after the addition of methanol, indicating that Zn-N-GDY has excellent methanol resistance.

[0061] In an O2-saturated electrolyte, a potential range including the oxygen reduction peak was selected to continuously scan 5000 CV cycles, and then the LSV curves before and after the cycle were compared. The results are shown in Figure 2. Figure 5 As described above, the results show that the LSV curve does not change significantly, indicating that the Zn-N-GDY prepared in Example 1 has good stability.

[0062] Experimental Example 3

[0063] The oxygen reduction reaction is a reaction involving multiple free radicals and intermediates, and has slow kinetics. There are two pathways for the oxygen reduction reaction, namely the 2-electron pathway and the 4-electron pathway. Compared with the 2-electron pathway, the 4-electron pathway has the following advantages: it provides a higher electromotive force and produces less H2O2 that undergoes a Fenton-like reaction with transition metals. Considering cost and battery efficiency, it is ideal to completely convert O2 into H2O, so it is more inclined to design an oxygen reduction catalyst with a 4-electron pathway. According to the LSV curve data of the test catalyst at different speeds, the KL equation can be used to calculate that the number of transferred electrons of the Zn-N-GDY prepared in Example 1 is about 3.8 to 3.9, indicating that the ORR reaction is indeed carried out through a 4-electron pathway.

[0064] Figure 6 Where a is the LSV curve of Zn-N-GDY prepared in Example 1 at different rotation speeds, b is the yield of H2O2 during the catalytic process, and c is the corresponding electron transfer number during the catalytic process.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a metal single atom doped nanocarbon material catalyst, characterized in that: include: Adding nitrogen-containing ligands and metal salts into solvent A, stirring and reacting to form complex MN; The nanocarbon material and the complex MN are dispersed in a solvent B and stirred for pre-adsorption; after the reaction is completed, the solvent B is removed to obtain a catalyst precursor; the catalyst precursor is first heated to 600-750° C. in an inert gas atmosphere, and then heated to 850-950° C. in a nitrogen atmosphere for calcination to obtain a metal single atom-doped nanocarbon material catalyst; Wherein, the nano-carbon material is nano-graphene or nano-hydrogen-substituted graphene.

2. The preparation method according to claim 1, characterized in that The metal salt is one of anhydrous ZnCl2, anhydrous FeCl3 or copper acetylacetonate; Alternatively, the nitrogen-containing ligand is one of pyrazole-3-carboxylic acid, urea, cyanamide, dicyandiamide or 2,2-bipyridine.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the metal salt to the nitrogen-containing ligand is 1:1 to 1:100, preferably 1:

10.

4. The preparation method according to claim 1, characterized in that: The time for stirring the reaction to form the complex MN is 20 to 30 hours.

5. The preparation method according to claim 1, characterized in that: Solvent A is ethanol or deionized water, and solvent B is an ethanol solution with a volume concentration of 20% to 100%. The preferred ethanol solution is a mixed solution of ethanol and deionized water.

6. The preparation method according to claim 1, characterized in that: The molar ratio of the metal salt to graphyne or hydrogen-substituted graphyne is 0.1% to 10%, preferably 1% to 2.5%.

7. The preparation method according to claim 1, characterized in that: The stirring time for pre-adsorption is 20 to 30 hours.

8. The preparation method according to claim 1, characterized in that: The calcination time is 0.5 to 2 hours, preferably 0.5 hours; Alternatively, during calcination, the heating rate is 1 to 10°C / min, more preferably 5°C / min.

9. A metal single atom doped nanocarbon material catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the metal single atom doped nanocarbon material catalyst according to claim 9 as an oxygen reduction working electrode catalyst or air electrode catalyst in a zinc-air fuel cell, a hydrogen-oxygen fuel cell, a magnesium-air fuel cell or an aluminum-air fuel cell.

Citation Information

Patent Citations

  • Preparation method of nitrogen-doped graphene-loaded metal monatomic catalysts

    CN107469855A

  • Nitrogen-doped graphdiyne riveted transition metal monatomic catalyst as well as preparation method and application thereof

    CN111384409A

  • Nitrogen-doped electrocatalyst, an preparation method and application thereof

    CN113224322A

  • Preparation method of iron and nitrogen co-doped gamma-graphdiyne carbon material

    CN115133045A

  • Preparation method of cobalt and nitrogen co-doped gamma-graphdiyne carbon material

    CN115448286A

Cited By

  • Preparation method of monatomic catalyst for oxygen reduction reaction

    CN119447325A

  • A method for preparing a single-atom catalyst for oxygen reduction reaction

    CN119447325B

  • Cobalt-doped three-dimensional porphyrin graphite monoalkyne catalyst as well as preparation method and application thereof

    CN121282224A