Coating process method of impulse turbine runner with beautiful appearance
By spraying two-component water-based polyurethane varnish or solvent-based acrylic polyurethane varnish on the turbine runner, combined with surface pretreatment and high-pressure airless spraying technology, the coating problem in beautifying the appearance of the turbine runner is solved, achieving a bright and bright appearance. The coating effect is plump, smooth and even, and the adhesion and anti-corrosion properties are improved, complying with environmental protection requirements.
Patent Information
- Application Number
- CN202410837393.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
The existing turbine runner has an unsightly appearance and lacks visual impact. During the beautification process, it is difficult to ensure that the coating is bright, plump, smooth, consistent in color, uniform in thickness, adhesion, flexibility and anti-corrosion properties. At the same time, it must be environmentally friendly and energy-saving. Require.
Use two-component water-based polyurethane varnish or solvent-based acrylic polyurethane varnish for spraying. Through surface pretreatment, selecting appropriate colors and process conditions, and using high-pressure airless spraying or air spraying technology to ensure the uniformity and adhesion of the coating, and Construction is carried out in a clean environment.
A bright, plump, flat and smooth coating with consistent color and uniform thickness is obtained. It has excellent adhesion and anti-corrosion properties, improves the visual effect and aesthetics of the runner, reduces the emission of harmful substances, and improves worker health. level.
Smart Images

Figure CN118751502A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating technology for a water turbine runner, and in particular to a coating technology method for an impulse water turbine runner with a beautified appearance. Background Art
[0002] At present, the appearance of most turbine runners on the market is the original color of stainless steel metal, with traces of polishing, lacking aesthetics and visual impact.
[0003] Therefore, the industry's R&D personnel considered spraying paint to beautify the runner to reflect the lines and contours of the runner, improving its visual effect and overall beauty while ensuring that the coating has excellent performance. However, in the specific implementation process, it was found that how to select suitable coating materials, colors and coating processes to ensure that the painted impulse turbine runner has beauty, the coating is bright, plump, smooth, consistent in color, and uniform in thickness, and at the same time has excellent adhesion on the smooth stainless steel runner surface, and the coating has excellent flexibility, elasticity and anti-corrosion properties, does not affect its normal use, and meets the current "environmental protection and energy saving" requirements. There is no research and application of the appearance spray painting beautification design and coating process methods for impulse turbine runners in this industry. Summary of the invention
[0004] The purpose of the present invention is to provide a coating process method for an impulse turbine runner with a beautified appearance, so as to obtain a runner with a bright, plump, smooth, uniform color and uniform thickness coating, and the coating has excellent adhesion on the smooth stainless steel runner surface, and is excellent in flexibility, elasticity and corrosion resistance.
[0005] The present invention is achieved through the following technical solutions:
[0006] A coating process for an impulse turbine runner with a beautified appearance comprises the following steps:
[0007] S1, select a paint material from two-component water-based polyurethane varnish and solvent-based acrylic polyurethane varnish for standby use;
[0008] S2. Paint in a clean, well-ventilated place with a wind speed of less than 0.5m / s. The temperature of the construction environment is 10-40℃, the humidity is ≤85%, the lighting illumination is ≥500Lux, and the surface temperature of the workpiece is 3℃ higher than the ambient dew point temperature.
[0009] S3. Pre-treat the surface of the wheel to be coated to remove the flaw detection fluid, cutting fluid, oil residue and dust on the surface until there is no oil stain when wiped with a white cloth or no crack when scratched with chalk;
[0010] S4. Determine the parts on the runner that need to be painted and those that do not need to be painted, and protect the parts that do not need to be painted;
[0011] S5, diluting the varnish in step S1 to a viscosity of 25 to 50 seconds using a 4-cup viscosity cup, filtering, and then applying the varnish using high-pressure airless spraying or air spraying;
[0012] S6. Paint film drying time is 24h or more, and coating thickness is 40-80μm.
[0013] Furthermore, in step S1, water-based polyurethane transparent blue varnish is selected, and the color numbers are: refer to the RAL standard color card, RAL5012 light blue, RAL5015 sky blue, RAL5017 traffic blue or refer to GSB05-1426-2001 "Paint Film Color Standard Sample Card", PB06 light blue, PB05 sea blue, PB11 peacock blue. Through color matching, stray light is eliminated, making the appearance color blue purer. The 60° gloss of the paint film is ≥80%, refer to GB / T9754-2007.
[0014] Furthermore, the coating of the varnish can withstand immersion in artificial seawater for ≥480 hours without blistering, peeling, rusting or cracking.
[0015] Furthermore, in step S2, a dedicated paint spraying purification room or a relatively closed purification place is used, and during the painting and paint drying period, the surface of the rotor should be protected from contact with dust and salt substances. Preferably, the cleanliness level of the paint spraying place reaches level 3 or above. Cleanliness level 3: The concentration of particulate matter in the air should be less than 10 million particles / cubic meter.
[0016] Furthermore, in step S4, for the parts that do not need to be painted, among which, the root area on the back side of the water bucket of the runner is evenly adhered with tape along the protection line at a consistent distance; the flange surface of the runner and the internal area of the water bucket are covered with kraft paper or plastic cloth and fixed with tape.
[0017] Furthermore, in step S5, the diluted varnish is filtered using a 100-180 mesh screen.
[0018] Furthermore, in step S5, when high-pressure airless spraying is adopted, the spraying distance is controlled to be 300-400 mm, the nozzle diameter of the spray gun is controlled to be 0.45-0.53 mm, the pressure ratio of the paint sprayer is controlled to be 30-40:1, and the spray width is controlled to be 300-400 mm.
[0019] Furthermore, in step S5, when air spraying is adopted, the compressed air is clean air after oil-water separation, the nozzle is 250-300 mm away from the workpiece surface, the nozzle diameter is 1.5-1.8 mm, and the air pressure is controlled to be 0.3-0.4 MPa.
[0020] Furthermore, during spraying, the nozzle is kept perpendicular to the surface of the wheel to be coated, and when the spray gun moves left and right, up and down, it needs to move at an equal distance from the coated surface, and the overlap of the paint spraying is 1 / 3 of the spray width.
[0021] Furthermore, in step S6, the dried coating has excellent adhesion on the smooth surface of the stainless steel wheel, and adheres to the surface of the wheel to reach level 1 or above by the cross-hatch method or ≥5MPa by the pulling method; the paint film has a flexibility of ≤1mm, and has no cracks, no mesh, and no damage; the coating has good elasticity, and when a hard object presses or a sharp object scratches the coating on the surface of the wheel, the coating can automatically rebound to its original appearance before being pressed or scratched after 10 to 15 seconds.
[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0023] 1. In the present invention, the coating method of this scheme can obtain a bright, full, smooth, uniform color and thickness coating. The coating has a certain anti-corrosion performance and can cover the grinding marks on the surface of the original stainless steel wheel, improving the visual effect and overall beauty of the wheel. In addition, environmentally friendly paint materials are preferred in this scheme, VOCs are reduced by more than 90%, and the occupational health level of workers during the construction process is improved.
[0024] 2. In the present invention, in step S1, the color of the coating used for the wheel is preferably transparent blue. Through color matching, stray light is eliminated, making the appearance color blue purer. Considering the use environment of the wheel, the coating material has excellent adhesion on the smooth stainless steel wheel surface, excellent flexibility, elasticity and anti-corrosion performance, can be dried naturally at room temperature, has good covering power, and excellent coating fullness. Two-component water-based polyurethane varnish and solvent-based acrylic polyurethane varnish coating can be selected. Environmentally friendly water-based polyurethane transparent blue varnish is preferred.
[0025] 3. In the present invention, the varnish used should have excellent atmospheric corrosion resistance. Preferably, the varnish is a material whose coating can withstand artificial seawater immersion for ≥480 hours without blistering, peeling, rusting, cracking, etc.
[0026] 4. In the present invention, in step S2, a dedicated spray paint purification room or a relatively closed purification place is used. During the painting and paint drying period, the surface of the wheel should be protected from dust and salt substances to avoid coating contamination and affect the coating quality. The cleanliness level of the spray paint place is grade 3 or above, and the cleanliness level 3 means that the concentration of particulate matter in the air should be less than 10 million particles / cubic meter.
[0027] 5. In the present invention, in step S4, it is necessary to design a suitable painting area in combination with the structure and functional requirements of the runner, that is, determine the painting range, and protect the area that does not need to be painted according to the design requirements. For the area at the root of the back of the water bucket that does not need to be painted, tape is used to stick evenly along the protection line at a consistent distance to ensure that the spraying effect of the root part that needs to be painted is consistent; for the non-painted parts such as the flange surface of the runner and the inside of the water bucket, kraft paper or plastic cloth is used to cover and fixed with tape to achieve the purpose of protecting the parts that do not need to be painted.
[0028] 6. In the present invention, in step S5, a 100-180 mesh screen is used to filter the diluted varnish to remove particles carried by the raw materials or carried by the materials during the preparation process, thereby ensuring the uniformity of the final coating and the quality of the coating.
[0029] 7. In the present invention, in step S5, a high-pressure airless spraying or air spraying process is used to ensure that the varnish is evenly coated on the surface of the runner without dead angles or omissions. During the spraying process, attention should be paid to controlling the viscosity of the coating and the spraying distance to obtain the best coating effect. When high-pressure airless spraying is used, the spraying distance is preferably controlled to 300-400mm, the nozzle caliber of the spray gun is controlled to 0.45-0.53mm, the pressure ratio of the paint sprayer is controlled to 30-40:1, and the spray width is controlled to 300-400mm; when air spraying is used, the compressed air is clean air after oil-water separation, the nozzle is 250-300mm away from the surface of the workpiece, the nozzle caliber is 1.5-1.8mm, and the air pressure is controlled to 0.3-0.4MPa.
[0030] 8. In the present invention, during spraying, the nozzle is kept perpendicular to the surface of the wheel being coated. When the spray gun moves left and right, up and down, it is necessary to move at an equal distance from the surface being coated, and avoid wrist rotation to form an arc movement to maintain uniform film thickness. The overlap of the spraying is 1 / 3 of the spray width.
[0031] 9. In the present invention, in step S6, the dried coating has excellent adhesion on the smooth surface of the stainless steel wheel, and adheres to the wheel surface to reach level 1 or above by the cross-hatch method or ≥5MPa by the drawing method; the paint film has a flexibility of ≤1mm, and has no cracks, no mesh, and no damage; the coating has good elasticity, and when a hard object presses or a sharp object scratches the coating on the wheel surface, the coating can automatically rebound to its original appearance before pressing or scratching after 10 to 15 seconds, further ensuring that the wheel itself is protected to a certain extent during storage and transportation, while keeping the color of the wheel surface unchanged, maintaining the glossiness for a long time, and maintaining its beautiful appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a three-dimensional effect diagram of a water turbine runner after coating obtained by adopting the coating process of this scheme in the present invention.
[0033] Figure 2 yes Figure 1 Top view of the . DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0035] Example 1
[0036] In order to facilitate the public to understand the present solution, this embodiment takes an impact turbine runner with a beautified appearance of the company as an example, and describes its coating method in detail in combination with the accompanying drawings.
[0037] A coating process method for an impact turbine runner with a beautified appearance, which relates to the technical field of coating process for turbine runners, comprises the following steps:
[0038] Step 1: Select a paint material from two-component water-based polyurethane varnish and solvent-based acrylic polyurethane varnish and set aside.
[0039] When implementing it specifically,
[0040] Ⅰ. For the color and gloss of the paint used for the runner: transparent blue paint is preferred, color number: refer to RAL standard color card, RAL5012 light blue, RAL5015 sky blue, RAL5017 traffic blue or refer to GSB05-1426-2001 "Paint Film Color Standard Sample Card", PB06 light blue, PB05 sea blue, PB11 peacock blue. Through color matching, stray light is eliminated, making the appearance color blue purer. The 60° gloss of the paint film is ≥80%, refer to GB / T9754-2007. The color and gloss of the runner surface must be consistent after spraying, and color difference visible to the naked eye is not allowed.
[0041] Ⅱ. Performance requirements for coating materials: The coating should have excellent adhesion, flexibility, elasticity and anti-corrosion properties, be able to dry naturally at room temperature, have good covering power and excellent coating fullness, such as two-component water-based polyurethane varnish and solvent-based acrylic polyurethane varnish.
[0042] The environmentally friendly water-based polyurethane transparent blue varnish is preferred, which has excellent atmospheric corrosion resistance and can withstand artificial seawater immersion for ≥480 hours without blistering, peeling, rusting, cracking, etc. The paint has excellent adhesion on the smooth surface of stainless steel runners.
[0043] Step 2: Paint in a clean, well-ventilated place with a wind speed of less than 0.5m / s. The temperature of the construction environment is 10-40℃, the humidity is ≤85%, the lighting illumination is ≥500Lux, and the surface temperature of the workpiece is 3℃ higher than the ambient dew point temperature.
[0044] In this step, it is preferred to use a dedicated paint spraying cleanroom or a relatively closed cleanroom. During the painting and paint drying period, the wheel surface should be free from dust and salt pollution. The paint spraying site should preferably be a cleanliness level of Grade 3 or above. Grade 3: The concentration of particulate matter in the air should be less than 10 million particles / cubic meter to avoid dust, salt and other substances from polluting the paint layer.
[0045] Step 3: Pre-treat the surface of the wheel to be coated. Completely clean the flaw detection fluid, cutting fluid, oil residue, dust and other pollutants. After cleaning, the surface cleanliness must be as follows: no oil stains when wiped with a white cloth or no cracks when scratched with chalk. Before spraying water-based paint, it is strictly forbidden to have impurities such as oil or cleaning agents on the surface of the workpiece to improve the adhesion of the coating.
[0046] Step 4: Determine the parts on the wheel that need to be painted and those that do not need to be painted, and protect the parts that do not need to be painted.
[0047] When implementing it, you need to first determine the scope of painting, refer to Figure 1 , 2 , design a suitable painting area according to the structure and functional requirements of the runner, and protect the areas that do not need to be sprayed according to the design requirements.
[0048] For areas on the back of the bucket that do not need to be painted, use tape to stick evenly along the protection line at a consistent distance to ensure consistent spraying effect at the root of the area that needs to be painted. For non-painted parts such as the runner flange surface and the inside of the bucket, cover them with kraft paper or plastic cloth and fix them with tape.
[0049] Step 5: Dilute the varnish in step 1 to a viscosity of 25 to 50 seconds using a 4-cup viscosity cup, filter, and then apply using high-pressure airless spray or air spray.
[0050] The specific steps are as follows:
[0051] S5.1. Weigh and mix the varnish according to the recommended proportion on the packaging barrel. The diluent for water-based varnish is industrial pure water, and the diluent for solvent-based varnish is the corresponding solvent diluent. The viscosity is adjusted to 25s~50s (Tu-4 cup viscosity cup) as needed;
[0052] S5.2. After the paint is diluted to a suitable viscosity, filter it with a 100-180 mesh screen;
[0053] S5.3, then use high-pressure airless spray or air spray process to ensure that the varnish is evenly coated on the wheel surface, without dead angles and omissions. During spraying, the nozzle is kept vertical to the surface of the wheel to be coated. When the spray gun moves left and right, up and down, it needs to move at an equal distance from the coated surface to avoid wrist rotation and arc movement to maintain uniform film thickness. The overlap of the spray paint is 1 / 3 of the spray width.
[0054] When high-pressure airless spraying is used, the spraying distance is preferably controlled to 300-400mm, the nozzle diameter of the spray gun is controlled to 0.45-0.53mm, the pressure ratio of the paint sprayer is controlled to 30-40:1, and the spray width is controlled to 300-400mm;
[0055] When air spraying is used, the compressed air is clean air after oil-water separation, the nozzle is 250-300mm away from the workpiece surface, the nozzle diameter is 1.5-1.8mm, and the air pressure is controlled at 0.3-0.4MPa.
[0056] Step 6: The paint film drying time is 24 hours or more, and the coating thickness is 40 to 80 μm.
[0057] In this step, the dried coating has excellent adhesion on the smooth surface of the stainless steel wheel, and adheres to the wheel surface to above level 1 of the cross-hatch method or ≥5MPa of the pulling method; the paint film has a flexibility of ≤1mm, and has no cracks, no mesh, and no damage; the coating has good elasticity, and when a hard object presses or a sharp object scratches the coating on the wheel surface, the coating can automatically rebound to its original appearance before pressing or scratching after 10 to 15 seconds, further ensuring that the wheel itself is protected to a certain extent during storage and transportation, while keeping the color of the wheel surface unchanged, maintaining the glossiness for a long time, and maintaining its beautiful appearance.
[0058] In the following specific implementation group, the above coating method was used, and its process parameters were adjusted according to the following Table 1 to obtain different coatings. The coatings obtained by each group were observed and tested, and the test results are shown in Table 2.
[0059] In this embodiment, the test methods and reference standards involved are as follows:
[0060] Paint film thickness: GB / T 13452.2 Determination of paint and varnish film thickness.
[0061] Resistance to artificial seawater immersion: GB / T 10834 Determination of salt water resistance of marine paints - Salt water and hot salt water immersion method.
[0062] Cross-cut method: GB / T 9286 Cross-cut test for paint and varnish films.
[0063] Paint film flexibility: GB / T 1731 Determination of paint film flexibility.
[0064] Hard object pressure recovery: When a hard object presses or a sharp object scratches the surface coating of the runner, how long will it take for the coating to automatically rebound to its original appearance before being pressed or scratched? The shorter the recovery time, the better the elasticity of the coating.
[0065] Table 1
[0066]
[0067] (Continued) Table 1
[0068]
[0069]
[0070] Table 2
[0071]
[0072]
[0073] It can be seen from the above-mentioned Examples 1-10 and Comparative Examples 1-3 that by strictly controlling the coating process conditions, a coating with excellent adhesion, flexibility, elasticity and corrosion resistance can be obtained on the smooth surface of the stainless steel runner, and the runner coating thickness is uniform, and the appearance is bright, plump, uniform in color, flat and smooth. The coating can further reflect the lines and contours of the runner, create a more dynamic visual effect, effectively improve the aesthetic appearance of the runner, and enhance the beauty and technological sense of the runner. It breaks through the current status of the coating technology for beautifying the appearance of non-impact stainless steel runners in the prior art. The coating can cover the grinding marks on the original stainless steel runner surface, refer to Figure 1 , 2 As shown, the visual effect and overall aesthetics of the runner are improved.
[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A coating process for an impulse turbine runner with a beautified appearance, characterized in that: The steps include: S1, select a paint material from two-component water-based polyurethane varnish and solvent-based acrylic polyurethane varnish for standby use; S2. Paint in a clean, well-ventilated place with a wind speed of less than 0.5m / s. The temperature of the construction environment is 10~40℃, the humidity is ≤85%, the lighting illumination is ≥500Lux, and the surface temperature of the workpiece is 3℃ higher than the ambient dew point temperature. S3. Pre-treat the surface of the wheel to be coated to remove the flaw detection fluid, cutting fluid, oil residue and dust on the surface until there is no oil stain when wiped with a white cloth or no crack when scratched with chalk; S4. Determine the parts on the runner that need to be painted and those that do not need to be painted, and protect the parts that do not need to be painted; S5, diluting the varnish in step S1 to a viscosity of 25-50s using a Tu-4 cup viscosity cup, filtering, and then applying the varnish using high-pressure airless spraying or air spraying; S6. Paint film drying time is 24h or more, and coating thickness is 40~80μm.
2. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S1, a water-based polyurethane transparent blue varnish is selected, and the color number is: refer to the RAL standard color card, RAL5012 light blue, RAL5015 sky blue, RAL5017 traffic blue or refer to GSB05-1426-2001 "Paint Film Color Standard Sample Card", PB06 light blue, PB05 sea blue, PB11 peacock blue, and the 60° gloss of the paint film is ≥80%.
3. The coating process for a Pelton turbine runner with a beautified appearance according to claim 2, characterized in that: The coating of the varnish can withstand immersion in artificial seawater for ≥480 hours without blistering, peeling, rusting or cracking.
4. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S2, a dedicated paint spraying purification room or a relatively closed purification place is used. During the painting and paint drying period, the surface of the wheel should be prevented from contacting dust and salt substances.
5. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S4, for the parts that do not need to be painted, among which, the root area of the back side of the water bucket of the runner is evenly pasted with tape along the protection line at a consistent distance; the flange surface of the runner and the internal area of the water bucket are covered with kraft paper or plastic cloth and fixed with tape.
6. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S5, the diluted varnish is filtered using a 100-180 mesh screen.
7. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S5, when high-pressure airless spraying is adopted, the spraying distance is controlled to be 300-400 mm, the nozzle diameter of the spray gun is controlled to be 0.45-0.53 mm, the pressure ratio of the paint sprayer is controlled to be 30-40:1, and the spray width is controlled to be 300-400 mm.
8. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S5, when air spraying is adopted, the compressed air is clean air after oil-water separation, the nozzle is 250-300 mm away from the workpiece surface, the nozzle diameter is 1.5-1.8 mm, and the air pressure is controlled to be 0.3-0.4 MPa.
9. The coating process for a Pelton turbine runner with a beautified appearance according to claim 7 or 8, characterized in that: During spraying, the nozzle should be kept perpendicular to the surface of the wheel to be coated. When the spray gun moves left and right, up and down, it needs to move at an equal distance from the coated surface, and the overlap area of the paint should be 1 / 3 of the spray width.
10. The coating process for a Pelton turbine runner with a beautified appearance according to claim 1, characterized in that: In step S6, the dried coating has excellent adhesion on the smooth surface of the stainless steel wheel, and adheres to the wheel surface to reach level 1 or above by the cross-hatch method or ≥5MPa by the pulling method; the paint film flexibility is ≤1mm, without cracks, mesh patterns, or damage; the coating has good elasticity, and when a hard object presses or a sharp object scratches the coating on the wheel surface, the coating can automatically rebound to its original appearance before pressing or scratching after 10 to 15 seconds.
Citation Information
Patent Citations
Casting painting process
CN105983525A
Oil paint coating construction method under high temperature and high humidity environment
CN107442369A
Locomotive coating method
CN108017976A
Water-based coating and preparing method and application thereof
CN111097670A
Varnish coating method for tank truck
CN112620052A