Transparent high-brightness silver coating for radar as well as preparation method and application of transparent high-brightness silver coating

By using a combination of low-content aluminum pigment and specific silver pearlescent pigment in the radar transparent coating, combined with solvent-based base material of high orientation agent, the problem of radar transparency and high brightness is solved, and the silver color with low loss and high brightness is achieved Coating effect simplifies process and improves performance.

CN119039840AActive Publication Date: 2024-11-29NIPPON PAINT CHINA

Patent Information

Application Number
CN202410609177.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-29
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

The prior art is difficult to take into account both the transparent and high-bright silver coating of radar. The combination of silver pearlescent pigment and aluminum pigment cannot effectively reduce radar transmission loss and maintain high brightness, resulting in general effects.

Method used

Use low-content aluminum pigments (≤1.5%) and specific silver pearlescent pigments (0.5-4.0%) to combine high-direction agent-content solvent-based base materials to control the proportion and dosage of aluminum pigments and silver pearlescent pigments to form a radar transparent High-brightness silver coating ensures that the sheet-like effect pigments are fully arranged, achieving high brightness, excellent angle-based heterochromaticity, flickering and hiding power.

Benefits of technology

The radar transmission loss is significantly reduced under the thinner dry film thickness, with an added value of <0.5dB, achieving high brightness and excellent metallic appearance, while simplifying the preparation process and improving process feasibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039840A_ABST
    Figure CN119039840A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent high-brightness silver coating for radar and a preparation method and application thereof. The high-brightness silver coating comprises at least one aluminum pigment, and the weight percentage of the aluminum pigment is less than or equal to 1.5%; at least one silver pearlescent pigment, the weight percentage of which is 0.5-4.0%; the solvent type base material is high in orientation agent content; wherein the weight percentage of the effective content of the orientation agent in the solvent type base material is greater than 5%. According to the invention, the aluminum pigment with low addition amount is matched with the silver pearlescent pigment with high covering performance to prepare the high-brightness transparent silver coating for the radar in a base material system with high orientation agent content, and the radar transmission loss increase < t > caused by the silver coating is reduced; 0.5 dB, and the optimal L15 degree gt; the silver coating prepared by the method has the advantages that the silver coating is more than 140, the silver coating also has excellent angle-dependent color variability, flickering property, covering power and obvious metallic appearance, and the silver coating is expected to be applied to use scenes with silver appearance requirements and radar signal transparency requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of radar transparent silver coatings, and more specifically to a radar transparent high-brightness silver coating, a preparation method and use thereof. Background Art

[0002] With the rapid development of autonomous driving technology, the use of millimeter wave radar (frequency 77-81GHz) is becoming more and more common. Each car or machine with autonomous driving function will be equipped with several radars, which are generally placed behind the bumper or corresponding parts. For coatings that do not contain metal components, their use will not interfere with radar signals. However, for metallic effect coatings with a silver appearance containing aluminum pigments, due to the high electrical conductivity of aluminum and the densely stacked layered structure, the penetration of radar signals is greatly affected, and the loss can reach more than 3dB, which brings challenges to the recognition of radar systems.

[0003] Silver pearlescent pigments with special coatings based on mica flakes or alumina substrates are another type of pigment that may achieve higher brightness, angular color change and glittering effects. CN103459515A discloses a pearlescent effect pigment with high hiding power and metallic appearance and high gloss silver appearance. A coating containing ilmenite is coated on the surface of a non-metallic flaky substrate. Through optimized formula and process technology, the pigment has excellent angular color change, brightness and glittering effects, and has a silver appearance similar to silver powder. CN1784476A discloses an interference pigment with high hiding power. It also coats a layer containing ilmenite on a flaky inorganic substrate, improves the problem of low hiding power of conventional pearlescent pigments, and has a silver-gray or silver metallic appearance. However, compared with aluminum pigments, such products still have the defects of low hiding power and insufficient metallic feel. At present, aluminum pigments cannot be completely replaced by pearlescent pigments. However, the dielectric properties of this inorganic oxide are not possessed by aluminum pigments.

[0004] CN116018291A discloses a radar-compatible coating containing metal effect pigments. The technical solution adopts a double-layer stacked structural design, one layer does not contain metal effect pigments, and the other layer contains metal effect pigments. The radar transmittance is improved by reducing the thickness of the metal pigment coating. However, the radar loss problem caused by the dense arrangement of aluminum pigments in the metal coating in the technical solution also exists. In addition, the double-layer structural design is complex in preparation and has low feasibility. The impact on properties such as hiding power and color tone is not disclosed. CN114222798A discloses a radar-transmissive coating composition using radar-transmissive pigments to replace metal aluminum pigments. At least 50% of the transmissive pigments are used to achieve the effect of reducing loss. However, the technical effect of this design is general, the minimum loss is controlled to be above 1.11dB, and there is a problem of insufficient brightness. At the same time, the impact on key properties such as scintillation and hiding power is not disclosed.

[0005] In summary, even if a compatible system of silver pearlescent pigments and aluminum pigments is used in the current existing technology, it is impossible to achieve a good balance between low radar transmission loss and high brightness. The results presented are generally mediocre. It is urgent to develop a more effective technical solution to improve the compatibility problem between radar transmission loss and high brightness. Summary of the invention

[0006] To solve the above problems, a first object of the present invention is to provide a radar transparent high brightness silver coating.

[0007] The second object of the present invention is to provide a method for preparing the high-brightness silver coating as described above.

[0008] The third object of the present invention is to provide a use of the high-brightness silver coating as described above applied to a plastic substrate.

[0009] In order to achieve the above first object, the present invention adopts the following technical scheme:

[0010] The invention discloses a radar transparent high-brightness silver coating, the high-brightness silver coating comprising

[0011] At least one aluminum pigment, the weight percentage of which is ≤1.5%;

[0012] At least one silver pearlescent pigment, the weight percentage of which is 0.5-4.0%; and

[0013] Solvent-based binders with high orienting agent content;

[0014] Wherein, the effective content of the orienting agent in the solvent-based base material is greater than 5% by weight.

[0015] Further, the silver pearlescent pigment is selected from a flaky substrate wrapped with iron oxide or titanium iron oxide;

[0016] The flaky substrate comprises one or more of mica flakes, mica flakes coated with titanium oxide, aluminum oxide flakes, titanium dioxide flakes, and glass flakes.

[0017] Further, the silver pearlescent pigment has a D50 of 5-30 μm and an average thickness of 100-500 nm;

[0018] The aluminum pigment has a D50 of 5-30 μm and a solid content of 65-75%.

[0019] Furthermore, the total weight percentage of the aluminum pigment and the silver pearlescent pigment in the high-brightness silver coating is controlled at 1.5-5.0%.

[0020] Furthermore, the weight ratio of the aluminum pigment to the silver pearlescent pigment is 1:0.5-4.

[0021] Furthermore, the dry film thickness of the high-brightness silver coating is 10-25 μm.

[0022] In order to achieve the above second purpose, the present invention adopts the following technical solutions:

[0023] The present invention discloses a method for preparing the high-brightness silver coating as described above, comprising the following steps:

[0024] Formulate solvent-based binders and pre-dispersed aluminum pigment dispersions and silver pearlescent pigment dispersions;

[0025] Adding the pre-dispersed aluminum pigment dispersion and the silver pearlescent pigment dispersion to the solvent-based base material, and mixing them evenly, a radar-transparent silver appearance coating is obtained;

[0026] The silver look paint is applied to a plastic substrate and allowed to cure.

[0027] In order to achieve the third object, the present invention adopts the following technical solutions:

[0028] The present invention discloses the use of a high brightness silver coating as described above applied to a plastic substrate.

[0029] Furthermore, the high-brightness silver coating is used on bumpers, automotive plastic parts or plastic substrates of other smart devices.

[0030] Further, the L15° value of the high brightness silver coating is above 125, preferably above 140, and more preferably above 145;

[0031] When the high-brightness silver coating is applied on a plastic substrate, the radar transmission loss increase caused by the high-brightness silver coating is less than 0.5 dB.

[0032] The beneficial effects of the present invention are as follows:

[0033] The present invention uses a compound of low-content aluminum pigment and a specific silver pearlescent pigment to ensure the reduction of radar transmission loss. When used in combination with a solvent-based base material containing a high content of a directing agent, the flaky effect pigment can be fully arranged, so that the obtained silver coating has high brightness, excellent angular heterochromaticity, scintillation, hiding power and obvious metallic appearance. The silver coating is expected to be used in scenes that require a silver appearance and at the same time require radar signal transparency.

[0034] The silver pearlescent pigment selected by the present invention is a flaky base pigment wrapped with iron oxide or titanium iron oxide, and is a pearlescent pigment with high hiding power and silver appearance wrapped with ilmenite components. It is a new type of pearlescent product, has the angular heterochromaticity, high brightness and glittering effect similar to aluminum pigment, and can make up for the influence of low content aluminum pigment to a certain extent.

[0035] The present invention controls the total addition amount of the aluminum pigment and the silver pearlescent pigment and the ratio between the two. On the one hand, the content of the solvent-based base material is implicitly specified, and the content of the orienting agent is further specified, so that the full arrangement of the flake effect pigment is guaranteed. On the other hand, through the usage relationship between the aluminum pigment and the silver pearlescent pigment, it is easier to obtain high brightness, excellent angular heterochromaticity, glitter, hiding power and obvious metallic appearance.

[0036] The high-brightness silver coating provided by the present invention can obtain good hiding power at a relatively thin dry film thickness (10-25 μm). When applied to a plastic substrate, the radar transmission loss increase caused by the high-brightness silver coating is less than 0.5 dB, and the radar transmission loss is significantly reduced. In addition, the preparation process of the high-brightness silver coating is simple, and there is no need for a double-layer stacked structure design as reported in the prior art, which is more feasible. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0038] Figure 1 A technical schematic diagram of the present invention in improving radar transparency is shown, wherein Figure 1 A is a coating formed by conventional metallic effect pigments, and B is a coating obtained by using the silver appearance coating of the present invention.

[0039] Figure 2 A cross-sectional SEM image of the high-brightness silver coating prepared in Example 6 of the present invention is shown.

[0040] Figure 3 A cross-sectional SEM image of the high-brightness silver coating prepared in Example 8 of the present invention is shown. DETAILED DESCRIPTION

[0041] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0042] As used herein, unless otherwise indicated, the term "part(s)" refers to parts by weight.

[0043] At present, the radars installed behind the bumper or other automotive plastic parts usually use frequencies of 24GHz or 77-81GHz. Among them, the 77-81GHz band radar is the most commonly used due to its small size, strong anti-interference ability, and policy access. Since its wavelength is in the millimeter wave band of 1-10mm, it is called millimeter wave radar. Millimeter wave radar has strong penetrating ability and can identify targets through plastic substrates (polypropylene, polycarbonate, etc.). However, as an electromagnetic wave, the energy of millimeter wave radar is not enough to penetrate metal media. For good conductors such as aluminum metal, the penetration depth of millimeter wave radar is only about a few hundred nanometers. See Figure 1 A in the middle is an aluminum effect coating commonly used in the automotive field, which generally contains about 1-6wt% aluminum pigment. The higher the content, the closer the aluminum powder tends to form a dense, continuous structure of pieces, and the multiple layers are superimposed, resulting in greater loss of millimeter waves when penetrating such a coating.

[0044] Aluminum pigment is a kind of flaky effect pigment obtained by grinding, generally with a size of 5-50μm and a thickness of about hundreds of nanometers. The outer surface generally has a variety of additives added during grinding, such as oleic acid. The aluminum pigment commonly used in automobiles is a silver dollar-shaped product with a size of 10-25μm. It has high brightness, delicate and strong metallic appearance, unique performance and is difficult to replace. The indispensability of aluminum pigments and the need to improve radar transmittance are contradictory. However, with the promotion and use of silver pearlescent pigments, new possibilities have been provided for the development of silver appearance coatings.

[0045] Pearlescent effect pigment is a kind of effect pigment prepared by coating a specific effect layer on the surface of an inorganic oxide flake substrate. Generally, the coating layer has a high refractive index, which interferes with the internal substrate to form a product with a specific effect. Pearlescent effect pigments include many categories, with corresponding products in various colors, sizes and various effects. They have been widely used in many fields, such as cosmetics, automobiles, home appliances, industrial equipment, etc. Pearlescent effect pigments have similar angle-dependent color, high brightness and glittering effects as aluminum pigments, but the hiding power is significantly lower. If silver pearlescent pigments are used alone, their metallic feel is not ideal.

[0046] In order to better obtain a silver appearance coating with low radar transmission loss and high brightness, silver pearlescent pigment and aluminum pigment can be compounded and used. There are two specific solutions based on this idea: the first solution is to design the aluminum pigment and the silver pearlescent pigment according to a double-layer structure, which are not affected by each other. Its advantage is mainly reflected in the fact that the arrangement of the two types of flaky effect pigments does not affect each other. However, the design of the double-layer structure will increase the complexity of the preparation process and is not conducive to construction. The second solution is to design the silver pearlescent pigment and the aluminum pigment according to a single-layer structure, that is, to mix the silver pearlescent pigment and the aluminum pigment into a uniform pigment. At this time, it is necessary to strictly control the amount of the two, both to reduce the influence of the arrangement of the two types of flaky effect pigments and to control the amount of aluminum pigment to reduce radar transmission loss. It is also necessary to consider the maintenance of brightness, angular color, glittering effect, metallic feel and covering power. However, it is actually very difficult to take both into account. Even obtaining a relatively balanced effect is very difficult for technicians.

[0047] On the basis of the second solution, in order to maintain the brightness and hiding power, technicians usually do not reduce the aluminum pigment too low, and its content is at least controlled at more than 2%, which is already the lower limit for technicians to develop aluminum pigment formulas. If the coating pursues radar transparency, that is, the radar loss caused by the coating is increased by less than 1dB, since technicians usually intuitively believe that as long as aluminum pigment is added, it will cause obvious radar loss and the radar transparency effect cannot be achieved, they generally directly develop single silver pearlescent pigments to completely replace aluminum pigments, or maintain the aluminum pigment above the lower limit of 2% to develop a composite formula of silver pearlescent pigments and aluminum pigments. They will not try to continue to reduce the aluminum pigment to develop a composite formula. This has become the inertial thinking of technicians. However, surprisingly, the inventors found that based on the coating system of the present invention, when a lower content of aluminum pigment (≤1.5%) is selected, there is almost no radar loss. On this basis, the present invention combines aluminum pigments and silver pearlescent pigments for use, see Figure 1 In B, a radar-transparent high-brightness silver coating is provided. The black ellipse represents aluminum pigment, and the white ellipse represents silver pearlescent pigment. The combination of the two reduces radar penetration loss. The high-brightness silver coating includes

[0048] At least one aluminum pigment, the weight percentage of which is ≤1.5%;

[0049] At least one silver pearlescent pigment, the weight percentage of which is 0.5-4.0%; and

[0050] Solvent-based binders with high orienting agent content;

[0051] Wherein, the effective content of the orienting agent in the solvent-based base material is greater than 5% by weight.

[0052] The use of aluminum pigment mainly ensures the metallic texture of the coating, which is irreplaceable by pearlescent pigments at this stage. However, considering the loss effect of aluminum pigment on radar transmittance, the weight percentage of aluminum pigment is controlled below 1.0% in the present invention. Affected by the addition amount, the radar loss of low-content aluminum pigment is significantly reduced.

[0053] In a specific embodiment, the aluminum pigment has a D50 of 5-30 μm and a solid content of 65-75%. The aluminum pigment contains a silver dollar shape, a corn flake shape or other suitable shapes. Currently, the aluminum pigment suppliers commonly used in automobiles include Toyo Aluminum, Star Platinum, and Zuxing. As an example, Toyo Aluminum's 4660NS (D50 is 9 μm) is used in the specific embodiment of the present invention. 4660NS has a delicate metallic feel, a high-brightness appearance, and excellent angular color performance, and is a representative product for automobiles.

[0054] Furthermore, the weight percentage of aluminum pigment in the high-brightness silver coating is ≤1.1%. Experiments have shown that the radar loss caused by the aluminum pigment at this addition amount is substantially negligible.

[0055] In order to eliminate the appearance problems such as decreased brightness caused by low-content aluminum pigments, the silver pearlescent pigment selected in the present invention is a flaky substrate pigment wrapped with iron oxide or titanium iron oxide, and the flaky substrate pigment includes one or more of mica flakes, mica flakes coated with titanium oxide, aluminum oxide flakes, aluminum oxide flakes coated with titanium oxide, titanium dioxide flakes, titanium dioxide flakes coated with titanium oxide, glass flakes, and glass flakes coated with titanium oxide; the D50 of the silver pearlescent pigment is 5-30μm, and the average thickness is 100-500nm. Pearlescent pigments with high hiding and silver appearance wrapped with ilmenite components are a new type of pearlescent product with similar angular heterochromaticity, high brightness and glittering effects as aluminum pigments. The main suppliers of the silver pearlescent pigment include Merck, Aika, Global New Materials and Kuncai Technology. In a specific embodiment, the silver pearlescent pigment is selected from 9602 (D50 is 15 μm), 9605 (D50 is 23 μm), 9612 (D50<15 μm) of the iriodin series of Merck and superfine (D50 is 13 μm), fine (D50 is 18 μm) and medium (D50 is 23 μm) of the OEM opaque silver series of Aika. However, these products still do not solve the hiding power problem caused by low content of aluminum pigments.

[0056] Furthermore, the total weight percentage of the aluminum pigment and the silver pearlescent pigment in the high-brightness silver coating is controlled at 1.5-5.0%. Exemplarily, the total weight percentage of the aluminum pigment and the silver pearlescent pigment in the high-brightness silver coating can be 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0057] Furthermore, the weight ratio of the aluminum pigment to the silver pearlescent pigment is 1:0.5-4. Exemplarily, the weight ratio of the aluminum pigment to the silver pearlescent pigment can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, etc. In a specific embodiment, when the weight ratio of the aluminum pigment to the silver pearlescent pigment is 1:1-2, it has higher brightness and lower radar transmission loss.

[0058] Brightness is represented by the L15° value close to the reflection angle, and the L15° value for the high brightness silver coating is at least above 125.

[0059] Orienting agents are a type of rheological additives that must be added to the coating system of flake effect pigments. Commonly used orienting agents include but are not limited to polyethylene wax, polyamide wax, ethylene vinyl acetate wax, butyl acetate cellulose, silicates, etc. The principle is to increase the viscosity and thixotropy of the coating system, enhance dispersion and prevent the flake effect pigments from sinking to the bottom. When drying, they can also support the arrangement of the flake effect pigments. In the coating system, about 1-5wt% of the orienting agent is generally added. In order to make up for the problem of poor hiding power of low-content aluminum pigments and silver pearlescent pigments, the effective content of the orienting agent is increased in the silver coating system of the present invention, and is controlled to be greater than 5% by weight, which is conducive to the full arrangement of the flake effect pigments to achieve high brightness and hiding power. The technician can further adjust the amount of the appropriate orienting agent according to different base material systems. For example, the weight percentage of the effective content of the orienting agent in the solvent-based base material can be controlled to be above 6%, above 7%, above 8%, above 9%, above 10%, above 11%, above 12% or above 13%.

[0060] The thickness of the high brightness silver coating obtained by the present invention is relatively thin, and its dry film thickness is 10-25 μm, preferably 10-20 μm. If there is no high content of directing agent to provide a role, the coating system of the present invention cannot achieve good hiding power with low content of aluminum pigment under the construction application of thinner coating. In a specific embodiment, the directing agent is selected from one or more of Eastman's CAB 531-1, Kusumoto Chemical's DISPARLON 4200-10 (active ingredient accounts for 10wt%), and BYK's CERAFAK 103. Eastman CAB 531-1 is a butyl acetate cellulose with a higher butyryl content than Eastman CAB381 cellulose ester. By combining butyl acetate cellulose with thermoplastic acrylic resin, a tough film with good scratch resistance and weather resistance can be obtained. Eastman CAB 531-1 and Eastman CAB 381 have similar hydroxyl content and solubility characteristics and are soluble in a variety of solvents. Eastman CAB 531-1 is a softer resin and requires less plasticizer modification than Eastman CAB 381 esters. DISPARLON 4200-10 is a non-soluble paste-like swelling dispersion fluid with dispersed oxidized polyethylene wax as the main component. It has little effect on the viscosity of the coating and is not easily affected by the type of pigment and medium. It can be used as a sedimentation inhibitor for almost all pigment dispersion coatings. It reacts with pigments, fillers, etc. in the coating to produce a stable colloidal structure that gives the coating excellent thixotropic properties, thereby preventing the sedimentation of the pigment and also preventing the coating from drooping. CERAFAK 103 is a dispersion of ethylene acrylic acid copolymer wax suitable for solvent-based effect coating systems. It can improve the orientation of effect pigments and reduce in-can sedimentation.

[0061] Acrylic resin, solvent and dispersant are also conventionally added to the solvent-based base. In a specific embodiment, the acrylic resin is selected from solvent-based acrylic resin, such as ACRYDIC ZHL-1063 and ACRYDIC WML-350 of DIC, accounting for 15wt% of the weight of the solvent-based base. The solvent is selected from xylene, ethyl acetate and isobutyl alcohol, and the oriented butyl acetate cellulose agent needs to be dispersed in advance with ethyl acetate and isobutyl alcohol to obtain its dispersion for use, and the dispersant is selected from BYK-192. Since the other materials in the solvent-based base except the oriented agent have little effect on the radar transmission loss, the technicians in this field replace the above products used as examples in the embodiment under the premise of ensuring the basic properties of the coating, and the increase in radar transmission loss caused by the different silver coatings obtained is basically equivalent.

[0062] The high-brightness silver coating developed by the present invention is obtained based on a solvent-based coating system, which can show lower radar loss, higher brightness, and excellent angular heterochromaticity, hiding power and scintillation effects. However, in the current development of water-based systems, the hiding power is low and the brightness is very low due to poor arrangement of aluminum pigments, and the technical effect is not obvious.

[0063] The present invention also provides a method for preparing the high-brightness silver coating as described above, comprising the following steps:

[0064] Formulate solvent-based binders and pre-dispersed aluminum pigment dispersions and silver pearlescent pigment dispersions;

[0065] Adding the pre-dispersed aluminum pigment dispersion and the silver pearlescent pigment dispersion to the solvent-based base material, and mixing them evenly, a radar-transparent silver appearance coating is obtained;

[0066] The silver appearance paint is applied to the plastic substrate containing the primer and allowed to cure.

[0067] Furthermore, the curing condition is baking at 60-80° C. for 20-30 minutes.

[0068] Furthermore, the thickness of the primer is 10-15 μm. The present invention further comprises a varnish layer coated on the high-brightness silver coating, and the thickness of the varnish layer is 30-40 μm.

[0069] The present invention also provides a use of the high-brightness silver coating as described above applied on a plastic substrate.

[0070] Furthermore, the high-brightness silver coating is used on bumpers, automotive plastic parts or plastic substrates of other smart devices.

[0071] Further, the L15° value of the high brightness silver coating is above 125, preferably above 140, and more preferably above 145;

[0072] When the high-brightness silver coating is applied to a plastic substrate, the radar transmission loss increase value caused by the high-brightness silver coating is less than 0.5 dB. In the present invention, the radar transmission loss increase value refers to the difference in radar transmission loss caused by adding aluminum pigment and silver pearlescent pigment to the high-brightness silver coating compared to before adding.

[0073] The following will be further explained in conjunction with the following specific scheme.

[0074] Solvent-based binder

[0075] The formulation of the solvent-based base material containing a high content of the orienting agent is also important for achieving the technical effect of the present invention. In order to illustrate the effect of the high content of the orienting agent, the present invention prepared two solvent-based base materials for comparative analysis: base material A and base material B, wherein base material A is a formulation containing a high content of the orienting agent, and base material B is a formulation containing a low content of the orienting agent.

[0076] Table 1 Solvent-based base material formula

[0077]

[0078]

[0079] Note: CAB 531-1 dispersion is prepared by dispersing CAB 531-1 in isobutyl alcohol and butyl acetate.

[0080] Coating requirements

[0081] Flex700 primer (Nippon Paint), color paint of the embodiment of the present invention and comparative example, and Flex200 / AP2000 varnish (Nippon Paint) were sprayed (ecogun spraying machine) on a 3mm thick PP plate (black, size 150*200mm) in sequence, with the thickness as shown in Table 2, and then placed flat in an oven and baked at 80°C for 30 minutes. The following index tests were then performed: the optical index was tested using a BYK-MAC tester, and the radar penetration loss was tested using a Rohde & Schwarz QAR device.

[0082] Table 2 Summary of coating information

[0083] coating Dry film thickness Flex700 Primer 10μm Silver appearance coating of the embodiment or comparative example of the present invention 20μm Flex200 / AP2000 Clearcoat 35μm

[0084] Comparative Examples 1-7

[0085] This group of comparative examples provides 7 formulations of silver appearance coatings, and the specific formulations are shown in Table 3.

[0086] Table 3

[0087]

[0088] The sample structure was prepared by using the formula provided in Table 3 and referring to Table 4, and then the radar transmission loss was tested under different sample structures. It can be seen from Table 4 that as the content of aluminum pigment decreases, the radar transmission loss decreases accordingly. When the content of aluminum pigment decreases to 1.5 parts (No. 5), the effect on the radar transmission loss is no longer obvious. When it continues to decrease to 1 part (No. 4), it has almost no effect on the radar transmission loss. Comparing the samples No. 1 and No. 2, the samples without any effect pigments have a slightly higher radar transmission loss than the pure PP board, which is due to the loss caused by the conductivity of the primer. In addition, by testing the samples No. 9 and No. 10, it was found that the silver pearlescent pigment 9602 and OEM superfine opaque silver almost do not produce radar transmission loss, indicating that it is feasible to use such materials in the development of radar transmission coatings.

[0089] Table 4

[0090] Serial number Sample structure Radar penetration loss / dB 1 PP board 0.88 2 PP board + FLEX700 primer 1.01 3 PP board + FLEX700 primer + base material A + FLEX200 varnish 0.99 4 PP board + FLEX700 primer + comparative example 1 + FLEX200 varnish 1.04 5 PP board + FLEX700 primer + comparative example 2 + FLEX200 varnish 1.22 6 PP board + FLEX700 primer + comparative example 3 + FLEX200 varnish 1.76 7 PP board + FLEX700 primer + comparative example 4 + FLEX200 varnish 3.2 8 PP board + FLEX700 primer + comparative example 5 + FLEX200 varnish 4.4 9 PP board + FLEX700 primer + comparative example 6 + FLEX200 varnish 0.99 10 PP board + FLEX700 primer + comparative example 7 + FLEX200 varnish 1.08

[0091] Comparative Examples 8-10

[0092] This group of comparative examples provides three formulas of silver appearance coatings, and the specific formulas are shown in Table 5.

[0093] Table 5

[0094] Components Comparative Example 8 / part Comparative Example 9 / part Comparative Example 10 / part Base A 60 / / Base material B / 60 60 Butyl acetate 35 35 35 4660NS 2.5 5 2.5 OEM medium opaque silver 2.5 / 2.5

[0095] Referring to the scheme of sequence number 8 in Table 4, the components of comparative examples 5 are replaced with those of comparative examples 8-10 to prepare the coating, and the brightness, angular heterochromaticity, scintillation, and hiding power are tested, and the effects of base material A and base material B on the performance of effect pigments are compared. The results are shown in Table 6. By comparing the schemes of sequence numbers 11 and 13, it can be seen that the FI of the coating of base material B decreases due to the addition of less directional agent, and L15° is significantly reduced, which is caused by the poor arrangement effect of the aluminum pigment. Therefore, even with the same amount of base material added, the hiding power of the base material B system will decrease. In addition, the granularity and scintillation of the coating also change, which may be caused by the aluminum sheets not being arranged in parallel and forming an angle. Under the system provided by the present invention, base material A containing a high content of directional agent is finally determined for subsequent experimental research.

[0096] Table 6

[0097]

[0098]

[0099] Examples 1-9

[0100] This group of examples provides 9 formulas of silver appearance coatings, and the specific formulas are shown in Table 7.

[0101] Table 7

[0102]

[0103] Referring to the solution of sequence number 8 in Table 4, the components of comparative example 5 were replaced with those of examples 1-9 to prepare the coating, and the brightness, angular heterochromaticity, scintillation, hiding power and radar transmission loss were tested. The results are shown in Table 8.

[0104] Table 8

[0105]

[0106] Note: No. 4, 8, 9, and 10 in Table 7 are used as the control group.

[0107] Result description:

[0108] Comparative Example 5 is a formula sample containing 5 parts (accounting for 5%) of aluminum pigment. From the results, it can be seen that it has excellent hiding power, brightness and scintillation performance. In addition, the metallic feel of the naked eye appearance is the best. Comparative Example 1 is a formula sample with a reduced amount of aluminum pigment to 1 part (accounting for 1.04%). Compared with Comparative Example 5, the hiding power is significantly reduced, the brightness is reduced, and the most important thing is that the metallic feel of the naked eye appearance is reduced. It is not as delicate and strong as Comparative Example 5. This may be because the aluminum pigment is already a discontinuous structure in the coating, and the decline in hiding power can be clearly found, and there are a lot of gaps. Although achieving the effect of radar transparency will cause a certain degree of loss of metallic feel, which is difficult to avoid, if the difference can be clearly observed by the naked eye, it will be difficult to meet the basic requirements of customers.

[0109] Comparative Examples 6 and 7 are samples prepared by selecting two silver pearlescent pigments used in the examples of the present invention to prepare samples without aluminum pigment. From the results, it can be seen that whether it is brightness, angle-dependent color effect or hiding power, they are all greatly different from those of Comparative Example 5, and the metallic feel is relatively low.

[0110] Examples 1-6 are samples prepared by mixing 4 parts of silver pearlescent pigments of different types with 1 part of aluminum pigment. Compared with Comparative Example 1, its hiding power is significantly improved, and the brightness of L45° is significantly improved, and the metallic sense of the naked eye appearance is significantly improved, but L15° is lower than Comparative Example 1, which may be because the silver pearlescent pigment covers the surface of the aluminum pigment, affecting the mirror reflection effect. In addition, the particle size of the silver pearlescent pigment has a regular effect on the results. Examples 4-6 show that the larger the particle size, the higher the L15° brightness, the higher the FI value, the slightly lower the hiding power, and the better the glittering effect. By adjusting the particle size used, products with corresponding indicators can be developed in a targeted manner.

[0111] Examples 7-8 are samples with adjusted amounts of aluminum pigment and silver pearlescent pigment, used to improve the problem of insufficient brightness in Examples 1-6. By reducing the amount of silver pearlescent pigment, it is found that L15° is significantly improved, and the brightness of L45° can still be maintained, with only a slight decrease in hiding power. In terms of comprehensive performance, Examples 7-8 are considered to be better examples.

[0112] Example 9 is a sample in which the aluminum pigment is further reduced to 0.5 parts (accounting for 0.5%). From the test results of radar transmission loss, it can be seen that further reducing the amount of aluminum pigment is not very meaningful for improving radar transmission loss, because 1 part (accounting for 1%) of aluminum pigment has almost no loss, and it is also found that the brightness, hiding power and other properties of Example 9 are significantly reduced, and the metallic appearance is also insufficient, indicating that in order to obtain a metallic silver appearance, a certain amount of aluminum pigment is necessary.

[0113] In summary, under the premise of ensuring radar transparency, the performance of the silver, metallic-appearance coating developed by the present invention is still excellent.

[0114] Performance Test 1

[0115] The cross-sectional SEM images of the coatings obtained from test numbers 19 and 21 are shown in Figure 2 and Figure 3 It can be found that the flake structures of the aluminum pigment and the silver pearlescent pigment are well arranged parallel to the coating. Since the coating No. 21 contains less silver pearlescent pigment, more gaps are found in the coating.

[0116] Performance Test 2

[0117] The glossiness and distinctness of image indexes of the coatings obtained from Nos. 4, 8, 19 and 20 were tested. The results are shown in Table 9. From the results, it can be seen that the addition of silver pearlescent pigment has no effect on the glossiness and distinctness of image indexes of the coatings.

[0118] Table 9

[0119]

[0120]

[0121] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A radar transparent high brightness silver coating, characterized in that: The high brightness silver coating comprises At least one aluminum pigment, the weight percentage of which is ≤1.5%; At least one silver pearlescent pigment, the weight percentage of which is 0.5-4.0%; as well as Solvent-based binders with high orienting agent content; Wherein, the effective content of the orienting agent in the solvent-based base material is greater than 5% by weight.

2. The high brightness silver coating according to claim 1, characterized in that: The silver pearlescent pigment is selected from a flaky substrate wrapped with iron oxide or titanium iron oxide; The flaky substrate comprises one or more of mica flakes, mica flakes coated with titanium oxide, aluminum oxide flakes, titanium dioxide flakes, and glass flakes.

3. The high brightness silver coating according to claim 1, characterized in that: The silver pearlescent pigment has a D50 of 5-30 μm and an average thickness of 100-500 nm; The aluminum pigment has a D50 of 5-30 μm and a solid content of 65-75%.

4. The high brightness silver coating according to claim 1, characterized in that: The total weight percentage of the aluminum pigment and the silver pearlescent pigment in the high-brightness silver coating is controlled at 1.5-5.0%.

5. The high brightness silver coating according to claim 4, characterized in that: The weight ratio of the aluminum pigment to the silver pearlescent pigment is 1:0.5-4.

6. The high brightness silver coating according to claim 1, characterized in that: The dry film thickness of the high-brightness silver coating is 10-25 μm.

7. The method for preparing a high-brightness silver coating according to any one of claims 1 to 6, characterized in that: The steps include: Formulate solvent-based binders and pre-dispersed aluminum pigment dispersions and silver pearlescent pigment dispersions; Adding the pre-dispersed aluminum pigment dispersion and the silver pearlescent pigment dispersion to the solvent-based base material, and mixing them evenly, a radar-transparent silver appearance coating is obtained; The silver look paint is applied to a plastic substrate and allowed to cure.

8. Use of the high brightness silver coating according to any one of claims 1 to 6 applied on a plastic substrate.

9. The use according to claim 8, characterized in that The high-brightness silver coating is used on bumpers, automotive plastic parts or plastic substrates of other smart devices.

10. The use according to claim 8, characterized in that The L15° value of the high brightness silver coating is greater than 125, preferably greater than 140, and more preferably greater than 145; The increase in radar transmission loss due to the high brightness silver coating is <0.5 dB.

Citation Information

Patent Citations

  • High-gloss silver-colored pigments having high covering power and a metal appearance, method for the production thereof and use of the same

    CN103459515A

  • Coating compositions, coatings, and coating systems for radar transmission and methods of making and using the same

    CN114222798A

  • Radar compatible coatings on substrates comprising metal effect pigments

    CN116018291A

  • Interference pigment with a high covering power

    CN1784476A

  • Plastics composition comprising at least one metal pigment, method for production and use thereof

    CN105612205A

Cited By

  • Metallic paint with high radar signal transparency, coating and use thereof

    CN123026954A