Preparation method of nickel-graphite sealing coating on surface of workpiece
By embedding microporous fillers in the nickel graphite coating, the problem that the nickel graphite coating is susceptible to impurity attack on the surface of the workpiece is solved, and the wear resistance and strength of the coating are significantly improved.
Patent Information
- Application Number
- CN202410858716.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The nickel graphite coating is easily attacked by impurities during the spraying process on the workpiece surface, affecting its wear resistance.
The microporous filler is embedded in the nickel graphite coating using an inlay machine. Through a vacuum environment and divided inlay process steps, the microporous filler is filled and solidified to enhance the coating strength and prevent impurity invasion.
The wear resistance and resistance to external damage of the nickel graphite coating are improved, and damage to the coating by impurities is avoided.
Smart Images

Figure CN118751504A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plating, and in particular relates to a method for preparing a nickel-graphite sealing coating on the surface of a workpiece. Background Art
[0002] Nickel graphite coating is a kind of abradable sealing coating with low hardness. Nickel graphite coating is widely used on the surface of aircraft engines, and plays a significant role in improving the overall efficiency of aircraft engines, reducing energy consumption and extending service life.
[0003] For example, the patent document with the publication number "CN116043291A" discloses a nickel-graphene composite coating with 310S stainless steel as the substrate and its preparation method, which relates to the field of metal plating technology. The nickel-graphene composite coating includes an electroplated nickel coating and an electroplated nickel-graphene composite coating; the raw materials of the electroplated nickel plating solution used for the electroplated nickel coating include nickel sulfamate, nickel chloride, citric acid, boric acid, and sodium dodecylbenzene sulfonate; the raw materials of the electroplated nickel-graphene composite plating solution used for the electroplated nickel-graphene composite coating include nickel sulfamate, nickel chloride, citric acid, boric acid, sodium dodecylbenzene sulfonate, and graphene. By adopting this patented technical solution, the nickel-graphene composite coating is firmly combined with the stainless steel substrate, so that the workpiece as a whole has better high-temperature oxidation resistance. However, through microscopic observation of nickel-graphite coating, it can be found that nickel-graphite coating is actually a microporous coating. When the nickel-graphite coating is sprayed on the surface of the workpiece, if impurities are mixed into the nickel-graphite coating, the impurities will destroy the nickel phase or graphite phase in the nickel-graphite coating and affect the wear resistance of the nickel-graphite coating. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a nickel-graphite sealing coating on the surface of a workpiece.
[0005] The present invention is achieved through the following technical solutions.
[0006] The present invention provides a method for preparing a nickel-graphite sealing coating on a workpiece surface, comprising the following steps:
[0007] Step 1: providing a workpiece and preparing a micropore filler;
[0008] Step 2: spraying the surface of the workpiece to obtain a nickel-graphite coating on the surface of the workpiece;
[0009] Step 3: embedding the micropore filler into the nickel graphite coating by an embedding machine.
[0010] The specific process steps of embedding the microporous filler into the nickel graphite coating by the embedding machine in step 3 are:
[0011] Step 1: placing the workpiece into a sealed container;
[0012] Step 2: extracting the gas in the sealed container by a vacuum pump to make the vacuum degree in the sealed container less than 100 kPa;
[0013] Step 3: Divide the micropore filler into two parts;
[0014] Step 4: In the sealed container, embedding the first portion of the micropore filler into the nickel graphite coating by an embedding machine;
[0015] Step 5: In the sealed container, embed the second micropore filler into the nickel graphite coating using an embedding machine.
[0016] The duration of implementing step 2 shall not be less than 16 minutes.
[0017] The mass ratio of the first microporous filler to the second microporous filler is 2:1.
[0018] The interval between implementing step 4 and step 5 shall be no less than 10 minutes.
[0019] The method for preparing the nickel-graphite sealing coating on the surface of a workpiece further comprises the following steps: after completing step three, the workpiece is stored in a room with an ambient temperature of 20° C. for at least 12 hours before taking the workpiece out.
[0020] The method for preparing the nickel-graphite sealing coating on the surface of the workpiece also includes the following steps: first immersing the workpiece in anhydrous ethanol for at least 20 minutes, then putting the workpiece into an oven for drying, and then performing step two.
[0021] The process parameters for putting the workpiece into the oven for drying are: the temperature in the oven does not exceed 60° C., and the drying duration is not less than 30 minutes.
[0022] The microporous filler in step 1 is prepared by uniformly mixing the following material components by mass for at least 1 minute: resin: 25 parts; curing agent: 3 parts.
[0023] The order of implementing step 1 and step 2 can be reversed.
[0024] The beneficial effect of the present invention is that: by adopting the technical scheme of the present invention, after the nickel graphite coating is sprayed on the surface of the workpiece, a microporous filler is embedded in the nickel graphite coating by an embedding machine, and the microporous filler is filled in the microporous structure inside the nickel graphite coating. On the one hand, it helps to enhance the strength of the nickel graphite coating itself and improve the ability of the nickel graphite coating to resist external force damage; on the other hand, it can prevent impurities in the external environment from invading the microporous structure inside the nickel graphite coating during the use of the workpiece, thereby improving the wear resistance of the nickel graphite coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0027] like Figure 1 As shown, the present invention provides a method for preparing a nickel-graphite sealing coating on a workpiece surface, comprising the following steps:
[0028] Step 1: providing a workpiece and preparing a micropore filler;
[0029] Step 2: spraying the surface of the workpiece to obtain a nickel-graphite coating on the surface of the workpiece;
[0030] Step 3: embed the micropore filler into the nickel graphite coating using an embedding machine.
[0031] By adopting the technical solution of the present invention, after the nickel graphite coating is formed by spraying on the surface of the workpiece, a microporous filler is embedded in the nickel graphite coating by an embedding machine. The microporous filler is filled in the microporous structure inside the nickel graphite coating. On the one hand, it helps to enhance the strength of the nickel graphite coating itself and improve the ability of the nickel graphite coating to resist external force damage; on the other hand, it can prevent impurities in the external environment from invading the microporous structure inside the nickel graphite coating during the use of the workpiece, thereby improving the wear resistance of the nickel graphite coating.
[0032] Specifically, the specific process steps of embedding the microporous filler into the nickel graphite coating by the embedding machine in step 3 are:
[0033] Step 1: Place the workpiece into a sealed container;
[0034] Step 2: Use a vacuum pump to evacuate the gas in the sealed container to make the vacuum degree in the sealed container less than 100 kPa; the duration of implementing step 2 is not less than 16 minutes. When implementing step 2, the vacuum degree in the sealed container is 86 kPa to 100 kPa.
[0035] Step 3: Divide the micropore filler into two parts;
[0036] Step 4: In a sealed container, embed the first portion of micropore filler into the nickel graphite coating by an embedding machine;
[0037] Step 5: In a sealed container, embed the second micropore filler into the nickel graphite coating using an embedding machine.
[0038] The mass ratio of the first microporous filler to the second microporous filler is 2:1. The interval between implementing step 4 and implementing step 5 is not less than 10min. The technical solution of the present invention is adopted, the microporous filler is divided into two parts, and is successively embedded in the nickel graphite coating. During the interval between step 4 and step 5, the microporous filler can be fully filled into the microporous structure inside the nickel graphite coating, thereby enhancing the strength of the nickel graphite coating itself, avoiding impurities in the external environment from invading the microporous structure inside the nickel graphite coating, and improving the wear resistance of the nickel graphite coating.
[0039] In addition, the method for preparing the nickel-graphite sealing coating on the surface of the workpiece further includes the following steps: after completing step 3, the workpiece is stored in a room with an ambient temperature of 20°C for at least 12 hours before the workpiece is used. Thus, the microporous filler is fully cured in the microporous structure of the nickel-graphite coating, the strength of the nickel-graphite coating itself is enhanced, impurities in the external environment are prevented from invading the microporous structure inside the nickel-graphite coating, and the wear resistance of the nickel-graphite coating is improved.
[0040] In addition, the preparation method of the nickel-graphite sealing coating on the surface of the workpiece also includes the following steps: first immersing the workpiece in anhydrous ethanol for at least 20 minutes, then putting the workpiece into an oven for drying, and then performing step two. The process parameters for putting the workpiece into the oven for drying are: the temperature in the oven does not exceed 60°C, and the drying duration is not less than 30 minutes. In step one, the microporous filler includes the following mass fractions of material components uniformly mixed for at least 1 minute: resin: 25 parts; curing agent: 3 parts. The implementation order of step one and step two can be interchanged. With the technical solution of the present invention, before spraying the nickel-graphite sealing coating on the surface of the workpiece, all dirt and impurities on the surface of the workpiece are first cleaned, which can avoid the negative impact of dirt and impurities on the generation process of the nickel-graphite coating. When the microporous filler is embedded, the workpiece and the microporous filler are always carried out in a vacuum environment, further avoiding the negative impact of dirt and impurities on the microporous structure of the nickel-graphite coating, thereby improving the strength and wear resistance of the nickel-graphite coating.
Claims
1. A method for preparing a nickel-graphite sealing coating on a workpiece surface, characterized in that: The following steps are involved: Step 1: providing a workpiece and preparing a micropore filler; Step 2: spraying the surface of the workpiece to obtain a nickel-graphite coating on the surface of the workpiece; Step 3: embedding the micropore filler into the nickel graphite coating by an embedding machine.
2. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 1, characterized in that: The specific process steps of embedding the microporous filler into the nickel graphite coating by the embedding machine in step 3 are: Step 1: placing the workpiece into a sealed container; Step 2: extracting the gas in the sealed container by a vacuum pump to make the vacuum degree in the sealed container less than 100 kPa; Step 3: Divide the micropore filler into two parts; Step 4: In the sealed container, embedding the first portion of the micropore filler into the nickel graphite coating by an embedding machine; Step 5: In the sealed container, embed the second micropore filler into the nickel graphite coating using an embedding machine.
3. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 2, characterized in that: The duration of implementing step 2 shall not be less than 16 minutes.
4. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 2, wherein: The mass ratio of the first microporous filler to the second microporous filler is 2:
1.
5. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 2, characterized in that: The interval between implementing step 4 and step 5 shall be no less than 10 minutes.
6. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 1, characterized in that: The method for preparing the nickel-graphite sealing coating on the surface of a workpiece further comprises the following steps: after completing step three, the workpiece is stored in a room with an ambient temperature of 20° C. for at least 12 hours before taking the workpiece out.
7. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 1, characterized in that: The method for preparing the nickel-graphite sealing coating on the surface of the workpiece also includes the following steps: first immersing the workpiece in anhydrous ethanol for at least 20 minutes, then putting the workpiece into an oven for drying, and then performing step two.
8. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 7, characterized in that: The process parameters for putting the workpiece into the oven for drying are: the temperature in the oven does not exceed 60° C., and the drying duration is not less than 30 minutes.
9. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 1, characterized in that: The microporous filler in step 1 is prepared by uniformly mixing the following material components by weight for at least 1 minute: resin: 25 parts; Curing agent: 3 parts.
10. The method for preparing a nickel-graphite sealing coating on a workpiece surface as claimed in claim 1, characterized in that: The order of implementing step 1 and step 2 can be reversed.
Citation Information
Patent Citations
Multi-component rod for hot spraying wearable sealing coating and preparation method thereof
CN101177770A
High-temperature abradable seal coating
CN101653998A
Metallographic detection method for flame sprayed NiCrAl / NiC coating
CN102798591A
Room-temperature curing coating with abradable sealing function and preparation method thereof
CN110982388A
Nickel-coated graphite sealing coating on surface of cast-iron workpiece, and preparation method of nickel-coated graphite sealing coating
CN111910144A