Arsenic alkali residue harmless treatment equipment and method
By designing harmless disposal equipment for arsenic-alkali slag, including antimony removal tanks, arsenic removal tanks, reaction kettles and roasting furnaces, full recovery of antimony, arsenic and alkali in arsenic-alkali slag has been achieved, solving resource problems in the existing technology. Problems of waste and environmental pollution are achieved by enabling a low-cost, waste-free treatment process.
Patent Information
- Application Number
- CN202410693263.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-11
AI Technical Summary
The existing technology fails to fully recover the active ingredients in the arsenic-alkali residue, resulting in resource waste and environmental pollution, and waste water, waste residue, and waste gas are produced during the treatment process.
A harmless disposal equipment for arsenic-alkali residue is designed, including an antimony removal tank, an arsenic removal tank, a reactor and a roasting furnace. Through water leaching, oxidation, reduction and other steps, arsenic, antimony and alkali are recovered, using multiple filtering devices and The stirring tank realizes the crushing and leaching of the suspended slurry, and finally it is reduced in the roasting furnace to obtain arsenic element.
It achieves full recovery of antimony, arsenic and alkali in arsenic-alkali residue, reduces waste generation, all raw materials can be recycled, has low processing cost, is suitable for large-scale promotion, and will not cause secondary pollution to the environment.
Smart Images

Figure CN118751669A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of arsenic-alkali slag treatment, and in particular to equipment and a method for harmless treatment of arsenic-alkali slag. Background Art
[0002] Arsenic alkali slag is a kind of hazardous solid waste produced by antimony smelting enterprises. In the process of pyrometallurgical antimony smelting in reverberatory furnace or blast furnace, crude antimony is refined by adding soda ash (sodium carbonate) or caustic soda (sodium hydroxide) to produce various types of refined antimony. The waste slag produced at the same time is called arsenic alkali slag. The main components of arsenic alkali slag are soda ash, arsenic and its compounds, antimony and its compounds. The content of the three substances is about: soda ash accounts for 53%, arsenic and its compounds account for 34%, and antimony and its compounds account for 11%. Arsenic and its compounds in arsenic alkali slag are highly toxic and easily soluble in water. If they are not properly stored, they are very likely to cause arsenic pollution incidents. Therefore, it is necessary to treat and recycle the arsenic alkali slag.
[0003] After searching, the Chinese patent publication number CN115491495A discloses a wet treatment process for harmless and resourceful treatment of arsenic alkali slag, wherein the arsenic alkali slag is leached in water to obtain leachate A and antimony-containing filter residue; the leachate A is evaporated and crystallized, and solid-liquid separation is performed to obtain sodium carbonate solid and liquid B; a ferrous solution is added to the leachate B to remove arsenic, and ferrous arsenate precipitate is obtained. The above patent can realize the separation of arsenic and alkali in arsenic alkali slag and the recovery of alkali, as well as direct arsenic removal under alkaline conditions, but the ferrous arsenate precipitate can only be disposed of by landfilling later, and this method does not fully recover the effective components in the arsenic alkali slag. The Chinese patent publication number CN113151687A discloses a method for treating arsenic alkali slag, comprising the following steps: mixing arsenic alkali slag or arsenic alkali slag leaching solution and a neutralizer to obtain a mixed solution, adding an oxidant to carry out an oxidation reaction, filtering to obtain solution A and filter residue A after the reaction is completed; adding solution A to a microwave reactor, adding an arsenic removal agent to remove arsenic, filtering to obtain a sulfate solution and filter residue, the method uses microwave-induced crystallization to achieve a removal and stabilization rate of arsenic in acidic wastewater and arsenic alkali slag of more than 99%, but the wastewater and waste residue generated by the method still need to be treated twice, and the effective components in the arsenic alkali slag are not fully recovered. In view of this, we propose a harmless treatment equipment and method for arsenic alkali slag. Summary of the invention
[0004] The purpose of the present invention is to provide a harmless treatment equipment for arsenic alkali slag, so as to carry out harmless treatment of arsenic alkali slag, reduce the generation of waste water, waste slag and waste gas, fully recycle the effective components in the arsenic alkali slag, and avoid secondary harm to the environment.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] On the one hand, the present invention provides harmless disposal equipment for arsenic alkali slag, including an antimony removal tank, a first filter device is connected to the bottom of the antimony removal tank, the bottom of the first filter device is connected to the arsenic removal tank through a pump and a pipeline, the top of the arsenic removal tank is connected to a lime milk storage tank through a pump and a pipeline, the bottom of the arsenic removal tank is connected to a second filter device, a reactor is arranged on one side of the second filter device, the bottom of the second filter device is connected to an alkali solution storage tank through a pump and a pipeline, the bottom of the alkali solution storage tank is connected to a third filter device, the bottom of the reactor is connected to a fourth filter device, a roasting furnace is arranged on one side of the fourth filter device, and the top of the roasting furnace is connected to an arsenic storage tank through a pipeline.
[0007] Preferably, a stirring tank is fixedly arranged inside the antimony removal tank, a accommodating chamber is formed between the stirring tank and the inner wall of the antimony removal tank, a plurality of through holes are evenly arranged on the upper part of the stirring tank, a cover body is threadedly connected to the top of the antimony removal tank, the cover body is sealingly abutted against the top of the stirring tank, a first motor is fixedly installed above the cover body, the output end of the first motor passes through the cover body and is fixedly connected to a knife shaft, the knife shaft is arranged inside the stirring tank, a plurality of blades are evenly arranged on the bottom of the knife shaft, a first water injection port and a hydrogen peroxide addition port are also opened on the cover body, and the first water injection port and the hydrogen peroxide addition port are communicated with the stirring tank.
[0008] Preferably, a second motor is provided on the top of the arsenic removal tank, and an output end of the second motor passes through the top wall of the arsenic removal tank and is connected to a first stirring paddle.
[0009] Preferably, a second water injection port is provided on one side of the top of the reactor, a third motor is fixedly provided on the top of the reactor, and an output end of the third motor passes through the top of the reactor and is connected to a second stirring paddle.
[0010] Preferably, the top of the arsenic storage tank is provided with an exhaust port, and the exhaust port is connected to a gas storage tank through a pipeline.
[0011] Preferably, valves are provided on the first water injection port, the hydrogen peroxide addition port, the second water injection port and the exhaust port.
[0012] On the other hand, the present invention provides a method for harmless disposal of arsenic alkali slag, using the above-mentioned harmless disposal equipment for arsenic alkali slag to treat the arsenic alkali slag, comprising the following steps:
[0013] S1, placing the arsenic alkali slag to be treated in an antimony removal tank, breaking it, immersing it in water, oxidizing it, filtering it to obtain antimony-containing filter residue and leaching liquid, and returning the antimony-containing filter residue to the refining furnace for further treatment;
[0014] S2, transferring the leachate in step S1 to a arsenic removal tank, adding sufficient amount of lime milk to react, and filtering to obtain alkaline solution and arsenic-containing filter residue;
[0015] S3, transferring the alkali solution in step S2 to an alkali solution storage tank, which contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace;
[0016] S4, transferring the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to a reactor, heating them, returning the temperature to room temperature after the reaction is complete, adding sufficient water to the reactor, stirring and filtering to obtain lime milk and arsenic-containing filter residue, and returning the lime milk to the lime milk storage tank for reuse;
[0017] S5, transferring the arsenic-containing filter residue in step S4 to a roasting furnace, adding a reducing agent to carry out a reduction reaction, and the arsenic vapor enters an arsenic storage tank to condense to obtain arsenic element.
[0018] Preferably, in step S1, the water immersion temperature is 40-55°C, the water immersion time is 60-120 min, the liquid-solid mass ratio is 3-6:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 1-5:10.
[0019] Preferably, in step S4, the heating temperature is 850-950° C., the heating time is 20-60 min, and the liquid-to-solid mass ratio is 1-5:3.
[0020] Preferably, the reaction temperature of the calcining furnace in step S5 is 700-1100°C, the reaction time is 40-80min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 1-3:10, the inside of the calcining furnace is an argon atmosphere, and the argon flow rate is 150-500mL / min.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The harmless disposal equipment for arsenic alkali slag includes an antimony removal tank, an arsenic removal tank, a reactor, and a roasting furnace. Antimony, arsenic and alkali in the arsenic alkali slag are recovered in turn, and the antimony-containing waste slag is returned to the refining furnace for further refining treatment. The recovered arsenic element can be used as an alloy additive and a doping element for semiconductor materials, and the recovered alkali liquor can be used for alkaline refining in the refining furnace.
[0023] 2. The antimony removal tank of the arsenic-alkali slag harmless disposal equipment is provided with a stirring tank, and a suspended slurry of the arsenic-alkali slag is formed inside the stirring tank. The blade will generate upward centrifugal force during the rotation process, driving the suspended slurry to move upward, and the suspended slurry with fine particles enters the containing chamber from the through hole, while the large particles of the arsenic-alkali slag continue to stay in the stirring tank for sufficient crushing. The antimony removal tank can fully leach the arsenic salts in the arsenic-alkali slag, thereby improving the leaching efficiency of the arsenic salts.
[0024] 3. The harmless disposal method of arsenic-alkali slag utilizes the harmless disposal equipment of the present invention to treat the arsenic-alkali slag, which can fully recover the antimony, arsenic and alkali in the arsenic-alkali slag without generating waste residue and wastewater, and all raw materials can be recycled. The method is simple, economical and will not generate secondary pollution.
[0025] 4. The harmless treatment method for arsenic alkali slag recycles more than 99% of the elemental arsenic, has good commercial value, and is worthy of commercial promotion.
[0026] 5. The reagents used in the harmless disposal method of arsenic alkali slag are simple, easy to obtain and low in price, which greatly reduces the treatment cost of arsenic alkali slag and is suitable for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a schematic diagram of the overall structure of the harmless treatment equipment for arsenic alkali slag of the present invention;
[0028] Figure 2 It is a schematic diagram of the internal structure of the antimony removal tank in the harmless treatment equipment for arsenic alkali slag of the present invention;
[0029] Figure 3 The present invention is a flow chart of the harmless treatment method of arsenic alkali slag.
[0030] In the figure: 1, antimony removal tank; 10, first filter device; 11, stirring tank; 111, through hole; 12, accommodating chamber; 13, cover; 131, first motor; 132, knife shaft; 133, blade; 134, first water injection port; 135, hydrogen peroxide addition port; 2, arsenic removal tank; 20, fourth filter device; 21, second motor; 22, first stirring paddle; 3, lime milk storage tank; 4, second filter device; 5, reactor; 51, second water injection port; 52, third motor; 53, second stirring paddle; 6, alkali solution storage tank; 7, third filter device; 8, arsenic storage tank; 81, exhaust port; 82, gas storage tank; 9, roasting furnace. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0033] In the description of this patent, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, it can be fixedly connected or set, or it can be detachably connected or set, or connected or set in one piece. For ordinary technicians in this field, the specific meanings of the above terms in this patent can be understood according to specific circumstances.
[0034] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "several" is two or more, unless otherwise clearly and specifically defined.
[0035] See also Figure 1-Figure 3 As shown, a technical solution provided by the present invention is:
[0036] Example 1
[0037] like Figure 1 , 2As shown, a harmless treatment equipment for arsenic alkali residue comprises an antimony removal tank 1, wherein the bottom of the antimony removal tank 1 is connected to a first filtering device 10 for separating antimony-containing residue, the bottom of the first filtering device 10 is connected to an arsenic removal tank 2 through a pump and a pipeline, the arsenic removal tank 2 is used to hold arsenic-containing leachate, the top of the arsenic removal tank 2 is connected to a lime milk storage tank 3 through a pump and a pipeline, the bottom of the arsenic removal tank 2 is connected to a second filtering device 4 for separating arsenic-containing residue and alkali solution, a reactor 5 is arranged on one side of the second filtering device 4, the calcium carbonate in the arsenic-containing residue is heated and decomposed into calcium oxide, the calcium oxide is reacted with water to generate lime milk, the bottom of the second filtering device 4 is connected to an alkali solution storage tank 6 through a pump and a pipeline, the alkali solution storage tank 6 is connected to the bottom of the second filtering device 4 through a pump and a pipeline, A third filtering device 7 is connected to the bottom of the tank 6. The lime milk in the alkali solution reacts with sodium carbonate to generate calcium carbonate precipitate, which is transferred to the reactor 5 together. The alkali solution is recovered for alkaline refining in the refining furnace. A fourth filtering device 20 is connected to the bottom of the reactor 5. The lime milk returns to the lime milk storage tank 3 for recycling. A roasting furnace 9 is provided on one side of the fourth filtering device 20. The top pipeline of the roasting furnace 9 is connected to an arsenic storage tank 8. The arsenic-containing filter residue is transferred to the roasting furnace 9 for reduction reaction to recover arsenic element. The recovered arsenic element can be used as an alloy additive and a doping element for semiconductor materials. The harmless disposal equipment for arsenic alkali slag does not generate waste residue and waste liquid, and the raw materials are recycled to the greatest extent.
[0038] In this embodiment, a stirring tank 11 is fixedly arranged inside the antimony removal tank 1, and the stirring tank 11 is used to hold the arsenic alkali slag to be treated. A accommodating chamber 12 is formed between the stirring tank 11 and the inner wall of the antimony removal tank 1, and a plurality of through holes 111 are evenly arranged in the middle and upper part of the stirring tank 11. A cover body 13 is threadedly connected to the top of the antimony removal tank 1, and the cover body 13 is sealed and abutted against the top of the stirring tank 11. A first motor 131 is fixedly installed above the cover body 13, and the output end of the first motor 131 passes through the cover body 13 and is fixedly connected to a knife shaft 132, and the knife shaft 132 is arranged inside the stirring tank 11, and a plurality of blades 133 are evenly arranged at the bottom of the knife shaft 132. The knife shaft 132 is driven to rotate, thereby driving the multiple blades 133 to rotate and break the arsenic alkali slag. The cover body 13 is also provided with a first water injection port 134 and a hydrogen peroxide addition port 135. The first water injection port 134 and the hydrogen peroxide addition port 135 are connected to the stirring tank 11. The arsenic alkali slag is soaked and broken at the same time, so that the arsenic alkali slag can be broken into finer particles, and a suspension slurry of the arsenic alkali slag is formed inside the stirring tank 11. The blade will generate an upward centrifugal force during the rotation process, driving the suspension slurry to move upward, and the fine-particle suspension slurry enters the containing chamber 12 from the through hole 111, while the large-particle arsenic alkali slag continues to stay in the stirring tank 11 for breaking. The antimony removal tank 1 can fully leach the arsenic salts in the arsenic alkali slag.
[0039] In this embodiment, a second motor 21 is provided on the top of the arsenic removal tank 2, and the output end of the second motor 21 passes through the top wall of the arsenic removal tank 2 and is connected to a first stirring paddle 22. The second motor 21 drives the first stirring paddle 22 to fully stir the suspension in the arsenic removal tank 2, so that all arsenic-containing salts are converted into arsenic-containing waste residues.
[0040] In this embodiment, a second water injection port 51 is provided on one side of the top of the reactor 5, and a third motor 52 is fixedly provided on the top of the reactor 5. The output end of the third motor 52 passes through the top of the reactor 5 and is connected to a second stirring paddle 53. Sufficient water is added to the reactor 5 through the second water injection port 51 to convert all the calcium oxide into lime milk. After filtration, the lime milk is returned to the lime milk storage tank 3 for recycling.
[0041] In this embodiment, an exhaust port 81 is provided at the top of the arsenic storage tank 8, and the exhaust port 81 is connected to a gas storage tank 82 through a pipeline. The arsenic vapor is cooled into arsenic element in the arsenic storage tank, and the gaseous carbon monoxide is transported to the gas storage tank 82 through a pipeline and finally burned.
[0042] In this embodiment, valves are provided on the first water injection port 134, the hydrogen peroxide addition port 135, the second water injection port 51, and the exhaust port 81 to facilitate the control of the arsenic-alkali slag treatment process.
[0043] Example 2
[0044] A method for harmless treatment of arsenic alkali slag, using the harmless treatment equipment for arsenic alkali slag of Example 1 to treat the arsenic alkali slag, comprising the following steps:
[0045] S1, placing the arsenic alkali slag to be treated in the antimony removal tank 1, breaking it, and then immersing and oxidizing it, filtering to obtain antimony-containing filter residue and leachate, and returning the antimony-containing filter residue to the refining furnace for further treatment, the immersion temperature is 40°C, the immersion time is 60min, the liquid-solid mass ratio is 3:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 1:10;
[0046] S2, transferring the leachate in step S1 to the arsenic removal tank 2, adding sufficient amount of lime milk to react, and filtering to obtain alkaline solution and arsenic-containing filter residue;
[0047] S3, transferring the alkali solution in step S2 to an alkali solution storage tank 6, which contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace;
[0048] S4, transferring the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to the reactor 5, heating, returning to room temperature after the reaction, adding sufficient water to the reactor 5, stirring, filtering to obtain lime milk and arsenic-containing filter residue, and returning the lime milk to the lime milk storage tank 3 for reuse, the heating temperature is 850° C., the heating time is 20 min, and the liquid-to-solid mass ratio is 1:3;
[0049] S5. The arsenic-containing filter residue in step S4 is transferred to a calcining furnace 9, and a reducing agent is added for reduction reaction. Arsenic vapor enters the arsenic storage tank 8 and condenses to obtain arsenic element. The reaction temperature of the calcining furnace 9 is 700° C., the reaction time is 40 min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 1:10, and the interior of the calcining furnace 9 is an argon atmosphere with an argon inlet flow rate of 150 mL / min.
[0050] In this embodiment, the arsenic content in the alkali solution recovered in step S3 is 0.8%, the arsenic content in the lime milk recovered in step S4 is 0.65%, and the arsenic content in the arsenic element recovered in step S5 is 99.02%.
[0051] Example 3
[0052] A method for harmless treatment of arsenic alkali slag, using the harmless treatment equipment for arsenic alkali slag of Example 1 to treat the arsenic alkali slag, comprising the following steps:
[0053] S1, placing the arsenic alkali slag to be treated in the antimony removal tank 1, breaking it, and then immersing it in water, oxidizing it, filtering it to obtain antimony-containing filter residue and leachate, and returning the antimony-containing filter residue to the refining furnace for further treatment, the immersion temperature is 45°C, the immersion time is 80min, the liquid-solid mass ratio is 4:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 2:10;
[0054] S2, transferring the leachate in step S1 to the arsenic removal tank 2, adding sufficient amount of lime milk to react, and filtering to obtain alkaline solution and arsenic-containing filter residue;
[0055] S3, transferring the alkali solution in step S2 to an alkali solution storage tank 6, which contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace;
[0056] S4, transferring the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to the reactor 5, heating, returning to room temperature after the reaction, adding sufficient water to the reactor 5, stirring, filtering to obtain lime milk and arsenic-containing filter residue, and returning the lime milk to the lime milk storage tank 3 for reuse, the heating temperature is 850° C., the heating time is 30 min, and the liquid-solid mass ratio is 2:3;
[0057] S5. The arsenic-containing filter residue in step S4 is transferred to a calcining furnace 9, and a reducing agent is added for reduction reaction. Arsenic vapor enters the arsenic storage tank 8 and is condensed to obtain arsenic element. The reaction temperature of the calcining furnace 9 is 800°C, the reaction time is 50 min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 1:10, and the interior of the calcining furnace 9 is an argon atmosphere, and the argon gas flow rate is 200-500 mL / min.
[0058] In this embodiment, the arsenic content in the alkali solution recovered in step S3 is 0.65%, the arsenic content in the lime milk recovered in step S4 is 0.62%, and the arsenic content in the arsenic element recovered in step S5 is 99.16%.
[0059] Example 4
[0060] A method for harmless treatment of arsenic alkali slag, using the harmless treatment equipment for arsenic alkali slag of Example 1 to treat the arsenic alkali slag, comprising the following steps:
[0061] S1, placing the arsenic alkali slag to be treated in the antimony removal tank 1, breaking it, and then immersing it in water, oxidizing it, filtering it to obtain antimony-containing filter residue and leaching liquid, and returning the antimony-containing filter residue to the refining furnace for further treatment, the immersion temperature is 50° C., the immersion time is 100 min, the liquid-solid mass ratio is 5:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 3:10;
[0062] S2, transferring the leachate in step S1 to the arsenic removal tank 2, adding sufficient amount of lime milk to react, and filtering to obtain alkaline solution and arsenic-containing filter residue;
[0063] S3, transferring the alkali solution in step S2 to an alkali solution storage tank 6, which contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace;
[0064] S4, transfer the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to the reactor 5, heat them, and restore them to room temperature after the reaction is completed, and add sufficient water to the reactor 5, stir and filter to obtain lime milk and arsenic-containing filter residue, and return the lime milk to the lime milk storage tank 3 for reuse, the heating temperature is 900° C., the heating time is 50 min, and the liquid-solid mass ratio is 4:3;
[0065] S5. The arsenic-containing filter residue in step S4 is transferred to a calcining furnace 9, and a reducing agent is added to carry out a reduction reaction. The arsenic vapor enters the arsenic storage tank 8 and is condensed to obtain arsenic element. The reaction temperature of the calcining furnace 9 is 1000° C., the reaction time is 70 min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 3:10, and the interior of the calcining furnace 9 is an argon atmosphere with an argon gas flow rate of 400 mL / min.
[0066] In this embodiment, the arsenic content in the alkali solution recovered in step S3 is 0.57%, the arsenic content in the lime milk recovered in step S4 is 0.58%, and the arsenic content in the arsenic element recovered in step S5 is 99.33%.
[0067] Example 5
[0068] A method for harmless treatment of arsenic alkali slag, using the harmless treatment equipment for arsenic alkali slag of Example 1 to treat the arsenic alkali slag, comprising the following steps:
[0069] S1, placing the arsenic alkali slag to be treated in the antimony removal tank 1, breaking it, and then immersing it in water, oxidizing it, filtering it to obtain antimony-containing filter residue and leachate, and returning the antimony-containing filter residue to the refining furnace for further treatment, the immersion temperature is 55° C., the immersion time is 120 min, the liquid-solid mass ratio is 6:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 5:10;
[0070] S2, transferring the leachate in step S1 to the arsenic removal tank 2, adding sufficient amount of lime milk to react, and filtering to obtain alkaline solution and arsenic-containing filter residue;
[0071] S3, transferring the alkali solution in step S2 to an alkali solution storage tank 6, which contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace;
[0072] S4, transferring the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to the reactor 5, heating, returning to room temperature after the reaction, adding sufficient water to the reactor 5, stirring, filtering to obtain lime milk and arsenic-containing filter residue, and returning the lime milk to the lime milk storage tank 3 for reuse, the heating temperature is 950° C., the heating time is 60 min, and the liquid-solid mass ratio is 5:3;
[0073] S5. The arsenic-containing filter residue in step S4 is transferred to a calcining furnace 9, and a reducing agent is added for reduction reaction. Arsenic vapor enters the arsenic storage tank 8 and is condensed to obtain arsenic element. The reaction temperature of the calcining furnace 9 is 1100° C., the reaction time is 80 min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 3:10, and the interior of the calcining furnace 9 is an argon atmosphere with an argon flow rate of 500 mL / min.
[0074] In this embodiment, the arsenic content in the alkali solution recovered in step S3 is 0.54%, the arsenic content in the lime milk recovered in step S4 is 0.55%, and the arsenic content in the arsenic element recovered in step S5 is 99.29%.
[0075] In summary, the harmless disposal equipment and method of arsenic alkali slag of the present invention can fully recycle the effective components in arsenic alkali slag, avoid waste of resources, and have low treatment costs. The treatment process will not produce wastewater, waste residue, and waste gas, and will not cause secondary harm to the environment. It is suitable for large-scale industrial promotion.
[0076] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A harmless treatment equipment for arsenic alkali slag, characterized in that: The invention comprises an antimony removal tank (1), wherein the bottom of the antimony removal tank (1) is connected to a first filtering device (10), the bottom of the first filtering device (10) is connected to an arsenic removal tank (2) via a pump and a pipeline, the top of the arsenic removal tank (2) is connected to a lime milk storage tank (3) via a pump and a pipeline, the bottom of the arsenic removal tank (2) is connected to a second filtering device (4), one side of the second filtering device (4) is provided with a reactor (5), the bottom of the second filtering device (4) is connected to an alkali liquid storage tank (6) via a pump and a pipeline, the bottom of the alkali liquid storage tank (6) is connected to a third filtering device (7), the bottom of the reactor (5) is connected to a fourth filtering device (20), one side of the fourth filtering device (20) is provided with a roasting furnace (9), and the top of the roasting furnace (9) is connected to an arsenic storage tank (8) via a pipeline.
2. The harmless treatment equipment for arsenic alkali slag according to claim 1 is characterized in that: A stirring tank (11) is fixedly arranged inside the antimony removal tank (1), a receiving chamber (12) is formed between the stirring tank (11) and the inner wall of the antimony removal tank (1), a plurality of through holes (111) are evenly arranged in the middle and upper part of the stirring tank (11), a cover body (13) is threadedly connected to the top of the antimony removal tank (1), the cover body (13) is in sealing contact with the top of the stirring tank (11), a first motor (131) is fixedly installed above the cover body (13), and the first The output end of the motor (131) passes through the cover body (13) and is fixedly connected to a knife shaft (132); the knife shaft (132) is arranged inside the stirring tank (11); a plurality of blades (133) are evenly arranged at the bottom of the knife shaft (132); a first water injection port (134) and a hydrogen peroxide addition port (135) are also provided on the cover body (13); the first water injection port (134) and the hydrogen peroxide addition port (135) are in communication with the stirring tank (11).
3. The harmless treatment equipment for arsenic alkali slag according to claim 1 is characterized in that: A second motor (21) is arranged on the top of the arsenic removal tank (2), and an output end of the second motor (21) passes through the top wall of the arsenic removal tank (2) and is connected to a first stirring paddle (22).
4. The harmless treatment equipment for arsenic alkali slag according to claim 1 is characterized in that: A second water injection port (51) is provided on one side of the top of the reactor 5. A third motor (52) is fixedly provided on the top of the reactor (5). The output end of the third motor (52) passes through the top of the reactor (5) and is connected to a second stirring paddle (53).
5. The harmless treatment equipment for arsenic alkali slag according to claim 1 is characterized in that: The top of the arsenic storage tank (8) is provided with an exhaust port (81), and the exhaust port (81) is connected to a gas storage tank (82) via a pipeline.
6. The harmless treatment equipment for arsenic alkali slag according to claim 1 is characterized in that: Valves are provided on the first water injection port (134), the hydrogen peroxide addition port (135), the second water injection port (51), and the exhaust port (81).
7. A method for harmless treatment of arsenic alkali slag, using the harmless treatment equipment for arsenic alkali slag according to any one of claims 1 to 6 to treat the arsenic alkali slag, characterized in that: The following steps are involved: S1, placing the arsenic alkali slag to be treated in the antimony removal tank (1), breaking it, immersing it in water, oxidizing it, filtering it to obtain antimony-containing filter residue and leaching liquid, and returning the antimony-containing filter residue to the refining furnace for further treatment; S2, transferring the leachate in step S1 to the arsenic removal tank (2), adding a sufficient amount of lime milk to react, and filtering to obtain an alkali solution and an arsenic-containing filter residue; S3, transferring the alkali solution in step S2 to an alkali solution storage tank (6), wherein the alkali solution storage tank (6) contains a sufficient amount of sodium carbonate solution, filtering to obtain alkali solution and calcium carbonate precipitate, and recovering the alkali solution for alkaline refining in a refining furnace; S4, transferring the arsenic-containing filter residue in step S2 and the calcium carbonate precipitate in step S3 to a reactor (5), heating them, and returning the temperature to room temperature after the reaction is complete, adding sufficient water to the reactor (5), stirring, and filtering to obtain lime milk and the arsenic-containing filter residue, and returning the lime milk to the lime milk storage tank (3) for reuse; S5, transferring the arsenic-containing filter residue in step S4 to a roasting furnace (9), adding a reducing agent to carry out a reduction reaction, and the arsenic vapor enters an arsenic storage tank (8) to be condensed to obtain arsenic element.
8. The harmless treatment method for arsenic alkali slag according to claim 7 is characterized in that: In the step S1, the water immersion temperature is 40-55°C, the water immersion time is 60-120 minutes, the liquid-to-solid mass ratio is 3-6:1, the oxidant is hydrogen peroxide, and the mass ratio of hydrogen peroxide to solid is 1-5:
10.
9. The harmless treatment method for arsenic alkali slag according to claim 7, characterized in that: In the step S4, the heating temperature is 850-950° C., the heating time is 20-60 min, and the liquid-to-solid mass ratio is 1-5:
3.
10. The harmless treatment method for arsenic alkali slag according to claim 7, characterized in that: The reaction temperature of the roasting furnace (9) in step S5 is 700-1100°C, the reaction time is 40-80min, the reducing agent is carbon element, the mass ratio of the reducing agent to the arsenic-containing filter residue is 1-3:10, the interior of the roasting furnace (9) is an argon atmosphere, and the argon flow rate is 150-500mL / min.
Citation Information
Patent Citations
Arsenic alkali residue treatment method
CN113151687A
Wet treatment process for harmlessness and recycling of arsenic alkali residues
CN115491495A