Working roll shifting method for reducing local high points of strip steel

By tracking the local high points of the strip cross section and the wear of the work rolls during the hot rolling production process, the work roll shifting motion is optimized, which solves the problem of local high points of the hot rolled strip cross section and improves production efficiency and product quality.

CN118751696APending Publication Date: 2024-10-11HUNAN VALIN LIANYUAN IRON & STEEL CO LTD

Patent Information

Application Number
CN202410968384.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively solve the problem of local high points in the cross section of hot-rolled strip steel, resulting in ribbing or corrugated defects during the rolling process, affecting production efficiency and the electromagnetic properties of the product.

Method used

By tracking the local high points of the strip cross-section during the hot rolling production process, statistics of work roll wear curves, setting the roll shifting interval and roll shifting step length, writing the roll shifting model, optimizing the work roll shifting motion, and reducing local Wear and avoid local high spots on the strip.

Benefits of technology

It effectively reduces the local high-point defects of the strip, improves the hot rolling production efficiency, avoids downstream batch ribbing, and extends the service life of the work rolls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751696A_ABST
    Figure CN118751696A_ABST
Patent Text Reader

Abstract

The invention discloses a working roll shifting method for reducing local high points of strip steel, which relates to the technical field of strip steel production, and comprises the following steps of: tracking hot rolling production, and determining whether local high points exist on the cross section of the strip steel at the last stage of a rolling unit; determining whether a single rolling unit is a rolling unit with a local high point or not; carrying out statistics on wear curves of working rollers of all racks in the rolling units with the local high points after the working rollers are discharged from the rolling units, and determining the racks with the working rollers with local wear; based on the convexity and the local high point of the hot-rolled strip steel finished product, a rack roll shifting interval and a roll shifting step length are set; the set data of the roll shifting interval and the roll shifting step length are written into a roll shifting model and put into use during production; according to the method, local abrasion of a working roller is reduced through reciprocating roll shifting of the local abrasion key rack working roller, and then the local high point defect of the cross section of rolled strip steel is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of strip steel production, and in particular to a working roll shifting method for reducing local high points of the strip steel. Background Art

[0002] The thickness of hot-rolled strip products is divided into the thickness in the length direction and the thickness in the width direction, of which the thickness in the width direction is also called the cross-sectional profile of the strip. As downstream users have higher requirements for product quality, the cross-sectional profile of hot-rolled strips has received increasing attention. For example, when there are local high points in the cross-sectional profile of hot-rolled silicon steel products, the cold rolling process is very likely to produce ribs or complex wave-shaped defects, which further affects the overall lamination effect of the downstream and ultimately affects the electromagnetic properties of the product.

[0003] The local high points of the strip are caused by the local wear of the rolls. As the number of rolled coils increases, the local wear of the rolls gradually increases, the local high points of the strip gradually increase, and the cross-sectional profile quality deteriorates. In severe cases, the machine must be stopped to replace the working rolls in advance, which reduces the rolling efficiency and increases the working roll consumption. At the same time, in order to ensure the rolling stability after the roll change, the strip thickness specification must be modified, resulting in the hot-rolled finished product being out of order. It can be seen that the deterioration of the cross-sectional profile of the strip is an important factor limiting production efficiency and needs to be addressed.

[0004] In the prior art, there are generally two ways to improve the local high points in the cross section of the strip: adopting a new working roll shape or reciprocating roll shifting of the downstream F5-F7 frames. However, the design, grinding and machine testing of the new roll shape affect the roll shape management and production scheduling of the grinding roll room. It is necessary to continuously adjust the roll shape curve through experimental conditions to optimize the working cycle. The reciprocating roll shifting of the working rolls of the downstream frames F5-F7 cannot avoid uneven wear of the upstream F1-F4 frames, and will eventually lead to the appearance of local high points in the cross section of the hot-rolled strip. Summary of the invention

[0005] The purpose of the present invention is to provide a method for reducing working roll shifting of local high points of strip steel, and to solve the following technical problems:

[0006] How to quickly improve the local high point phenomenon caused by the working rolls of the upstream and downstream stands on the strip.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for reducing working roll shifting at a local high point of a strip steel comprises the following steps:

[0009] S1: Track hot rolling production to determine whether there are local high points in the cross section of the strip at the end of the rolling unit;

[0010] S2: confirm whether a single rolling unit is a rolling unit with a local high point;

[0011] S3: Counting the wear curves of the working rolls of each stand after they are removed from the mill in multiple rolling units with local high points, and determining the stands with local wear on the working rolls;

[0012] S4: Based on the convexity and local high points of the hot-rolled strip finished product, the roll shifting interval and the roll shifting step length of the stand are set;

[0013] S5: Write the setting data of the roll shifting interval and the roll shifting step length in step S4 into the roll shifting model and put it into use during production.

[0014] In a further embodiment of the present invention: in step S1, the method for determining whether there is a local high point in the cross section of the strip is:

[0015] Checking the cross-sectional data of the strip, the strip thickness gradually increases from the edge to the middle, and the local maximum value h1 of the strip thickness appears at amm away from the operating side / transmission side edge of the strip; the local minimum value h2 of the strip thickness appears at amm away from the operating side / transmission side edge of the strip. When (h1-h2)>xum, it is considered that there is a local high point on the operating side / transmission side edge of the strip, where x is the maximum allowable local high point.

[0016] In a further embodiment of the present invention: the local high point is located near the edge of the steel strip and appears on one side or both sides of the steel strip.

[0017] In a further solution of the present invention: in step S2, the method for determining whether a single rolling unit is a rolling unit with a local high point is:

[0018] When the number of steel coils to be rolled in a single rolling unit is N, and a local high point appears in the cross-section of the strip when rolling the nth roll of strip, and the local high point still exists after subsequent manual adjustment, and (n / N) < y, this rolling unit is considered to be a rolling unit with local high points in the cross-section of the strip; where y is the minimum proportion of normal coils with local high points in a single plan.

[0019] In a further solution of the present invention: in step S3, the method for determining whether the working roll is a rack with local wear is:

[0020] Looking back at the wear curve of the working roll after it was removed from the machine, the edge wear of the working roll wear area is w1, and the middle wear is w2. When w1>w2, it indicates that the edge wear is greater than the middle wear, that is, there is local wear on the edge of the working roll wear area of ​​the frame.

[0021] In a further solution of the present invention: in step S4, the roller shifting interval and roller shifting step length are used to avoid the finished strip steel having a small convexity and to reduce the local high points of the strip steel by reducing the wear of the working rolls.

[0022] In a further solution of the present invention: in step S5, the setting data of the roll shifting is input into the rolling model in the form of numerical values, and during the production process, the specific stand reciprocates the roll shifting according to the set roll shifting value.

[0023] Beneficial effects of the present invention:

[0024] The method for reducing working roll shifting of local high points of strip steel of the present invention is mainly achieved by tracking the local high points of the cross-section of the strip steel of a certain rolling unit in the hot rolling production process, confirming whether there are local high points in a single rolling unit, counting the wear curves of the working rolls of multiple rolling units with local high points after leaving the machine, determining the frame with serious local wear of the working rolls, setting the roll shifting interval and the roll shifting step length of the frame based on the convexity of the finished hot-rolled strip steel and the local high points, writing the roll shifting setting data into the roll shifting model and putting it into use during production. The local wear of the working rolls can be reduced by the reciprocating roll shifting of the working rolls of the frame with emphasis on local wear, thereby reducing the local high point defects in the cross-section of the strip steel after rolling. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 is a local high point curve diagram of the cross section of the strip steel at the end of the rolling unit before optimization in one embodiment of the present invention;

[0027] Figure 2 It is a wear curve diagram of working rolls after F3 and F4 are removed from the mill when there are local high points in the rolling unit before optimization in one embodiment of the present invention;

[0028] Figure 3 This is a data diagram of the roll shifting of F3 and F4 working rolls before optimization in one embodiment of the present invention;

[0029] Figure 4 This is a data diagram of the roll shifting of the F3 and F4 working rolls after optimization in one embodiment of the present invention;

[0030] Figure 5 is a local high point curve diagram of the cross section of the strip steel at the end of the rolling unit after optimization in one embodiment of the present invention;

[0031] Figure 6 This is a wear curve diagram of the working rolls of F3 and F4 after being optimized in one embodiment of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The present invention discloses a working roll shifting method for reducing local high points of a steel strip, which is explained in detail below in conjunction with an actual hot rolling production process.

[0034] In the actual production process of the hot rolling unit, a total of 7 stands are arranged, namely F1-F7, each stand is provided with two working rolls for rolling the strip steel, and the strip steel is rolled by the working rolls in the F1-F7 stands in turn.

[0035] The first step is to track the hot rolling production process and determine whether there is a local high point in the cross-section of the strip at the end of the rolling unit; check the cross-sectional data of the strip, the thickness of the strip gradually increases from the edge to the middle, and the local maximum value h1 of the strip thickness appears at amm away from the edge of the operating side / transmission side of the strip; the local minimum value h2 of the strip thickness appears at amm away from the edge of the operating side / transmission side of the strip. When (h1-h2)>xum, it is considered that there is a local high point on the edge of the operating side / transmission side of the strip, where x is the maximum allowable value of the local high point.

[0036] Take one of the strip steel rolls as an example. Figure 1 As shown, firstly, the local high point situation on the transmission side of the strip is analyzed. The local maximum value of 2478.4um appears in the thickness of the strip at a position 44mm away from the edge of the transmission side of the strip, then h1=2478.4um, and the local minimum value of 2472.9um appears at a position 88mm away from the edge of the transmission side of the strip, then h2=2472.9um, therefore, the local high point value of the transmission side of the strip is h1-h2=5.5um; then the same method is used to obtain the local high point value of 5.1um on the operating side of the strip; according to the downstream cold rolling production capacity, the local high point allowable value x is set to 5um, and the larger local high point value between the operating side and the transmission side of the strip is taken, that is, the local high point value of the transmission side of the strip is 5.5um, 5.55um>5um, so it can be judged that there is a local high point in the cross section of this roll of strip.

[0037] The second step is to confirm whether there are local high points in a single rolling unit; when the number of steel coils to be rolled in a single rolling unit is N, a local high point appears in the cross-section of the strip when the nth roll of strip is rolled, and the local high point still exists after subsequent manual adjustment, and (n / N) < y, this rolling unit is considered to be a rolling unit with local high points in the cross-section of the strip; where y is the minimum proportion of normal coils with local high points in a single plan.

[0038] For example, in an embodiment of the present invention, during normal planned production, the number of steel coils to be rolled in a single rolling unit is 55, that is, N=55; in order to avoid excessive local high points exceeding the standard number of coils, which will lead to subsequent batch ribs, the minimum proportion y of steel coils in which there are no local high points in the cross-section of the strip in a single rolling unit is set to 0.9; taking the rolling unit of this embodiment as an example, after rolling 32 coils, there are local high points in the cross-section of the strip, and the local high points still exist after subsequent manual adjustment, that is, n=32; since n / N=32 / 55=0.58<0.9, this rolling unit is considered to be a rolling unit with local high points.

[0039] The third step is to count the wear curves of the working rolls of each stand in multiple rolling units with local high points after they are removed from the machine, and determine the stands with local wear on the working rolls; check the wear curves of the working rolls after they are removed from the machine, the edge wear amount of the working roll wear area is w1, and the middle wear amount is w2. When w1>w2, it indicates that the edge wear amount is greater than the middle wear amount, that is, there is local wear on the edge of the working roll wear area of ​​the stand.

[0040] See also Figure 2 Taking F3 and F4 frames as examples, the edge wear of the working roll wear area of ​​F3 frame is 0.055mm, that is, w1=0.055mm, and the middle wear is 0.046mm, that is, w2=0.046mm; the edge wear of the working roll wear area of ​​F4 frame is 0.059mm, that is, w1=0.059mm, and the middle wear is 0.031mm, that is, w2=0.031mm; both F3 and F4 frames have the situation of w1>w2, that is, the edge wear of the working roll is greater than the middle wear, so the working rolls of F3 and F4 frames have local wear.

[0041] The fourth step is to set the roll shifting range and step length of the stand based on the convexity and local high points of the hot-rolled strip finished product.

[0042] See also Figure 3 Before the optimization, the shifting positions of the working rolls of the F3 and F4 frames were adjusted by the operators according to the production situation, resulting in the shifting positions remaining unchanged for a long time.

[0043] In order to make the working rolls of F3 and F4 frames wear evenly and avoid the finished strip convexity being too small, the working rolls of F3 and F4 frames are set to reciprocating roll shifting with a roll shifting interval of -(30-60) mm. The roll shifting step lengths at different positions are planned as follows: Figure 4 shown.

[0044] In the fifth step, the setting data of the roll shifting interval and the roll shifting step length in the fourth step are written into the roll shifting model and put into use during production; the setting data of roll shifting is input into the rolling model in numerical form, and during the production process, the specific frame shifts the rolls back and forth according to the set roll shifting value.

[0045] In an embodiment of the present invention, the roll shifting setting data of the above-mentioned F3 frame and F4 frame are written into the roll shifting module of the secondary plate shape model and put into use at the initial stage of planned rolling. When the optimized roll shifting model is used for production, the local high points of the strip are significantly improved.

[0046] See also Figure 5 , the local high point situation of the strip cross section after optimizing the roller shifting of F3 frame and F4 frame has been significantly improved;

[0047] See also Figure 6 The wear of the working rolls of the F3 and F4 frames after they are optimized and shifted is significantly improved.

[0048] Working principle of the present invention:

[0049] The present invention adopts the above-mentioned roll shifting method, which reduces the local high points of the working rolls, improves the local high points of the strip during the rolling process, increases the number of single planned coils for hot rolling, and avoids downstream batch rib reduction while improving hot rolling production efficiency.

[0050] In the description of the present invention, it should be understood that the terms "upper", "lower", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction and a specific direction structure and operation, and therefore, cannot be understood as a limitation on the present invention. In addition, "first" and "second" are only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.

[0051] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for reducing working roll shifting at local high points of strip steel. It is characterized in that The following steps are involved: S1: Track hot rolling production to determine whether there are local high points in the cross section of the strip at the end of the rolling unit; S2: confirm whether a single rolling unit is a rolling unit with a local high point; S3: Counting the wear curves of the working rolls of each stand after they are removed from the mill in multiple rolling units with local high points, and determining the stands with local wear on the working rolls; S4: Based on the finished convexity and local high points of the hot-rolled strip, the roll shifting interval and the roll shifting step length of the stand are set; S5: Write the setting data of the roll shifting interval and the roll shifting step length in step S4 into the roll shifting model and put it into use during production.

2. The method for reducing work roll shifting of local high points of strip steel according to claim 1, It is characterized in that In step S1, the method for determining whether there is a local high point in the cross section of the strip is: Check the cross-sectional data of the strip. The strip thickness gradually increases from the edge to the middle. The strip thickness reaches a local maximum value h at a distance of amm from the edge of the strip operation side / transmission side. 1 ; The strip thickness has a local minimum value h at the position bmm away from the edge of the strip operation side / transmission side 2 , when (h 1 -h 2 )>xum, it is considered that there is a local high point on the operating side / transmission side of the strip, where x is the maximum allowable value of the local high point.

3. The method for reducing work roll shifting of local high points of strip steel according to claim 1, It is characterized in that The local high point is located near the edge of the steel strip and appears on one side or both sides of the steel strip.

4. The method for reducing work roll shifting of a local high point of a strip according to claim 1, It is characterized in that In step S2, the method for determining whether a single rolling unit is a rolling unit with a local high point is as follows: When the number of steel coils to be rolled in a single rolling unit is N, and a local high point appears in the cross-section of the strip when rolling the nth roll of strip, and the local high point still exists after subsequent manual adjustment, and (n / N) < y, this rolling unit is considered to be a rolling unit with local high points in the cross-section of the strip; where y is the minimum proportion of normal coils with local high points in a single plan.

5. The method for reducing work roll shifting of local high points of strip steel according to claim 1, It is characterized in that In step S3, the method for determining whether the working roll is a rack with local wear is as follows: Check the wear curve of the working roll after it leaves the machine. The wear amount of the edge of the working roll wear area is w 1 , the wear amount in the middle is w 2 , when w 1 >w 2 When , it indicates that the wear on the edge is greater than that in the middle, that is, there is local wear on the edge of the working roll wear area of ​​the frame.

6. The method for reducing work roll shifting of a local high point of a strip according to claim 1, It is characterized in that In step S4, the roll shifting interval and the roll shifting step length are used to avoid the finished strip steel having a small convexity and to reduce the local high points of the strip steel by reducing the wear of the working rolls.

7. The method for reducing work roll shifting of local high points of strip steel according to claim 1, It is characterized in that In step S5, the setting data of the roll shifting is input into the rolling model in the form of numerical values, and during the production process, the specific stand reciprocates the roll shifting according to the set roll shifting value.

Citation Information

Patent Citations

  • Hot rolling high-order curve work roll shifting strategy control taking both wave shape and section into consideration

    CN105598183A

  • Intelligent roller channeling method for working rollers of hot continuous rolling mill

    CN108273853A

  • Asynchronous double-attenuation roll shifting control method for hot-rolled sheet working rolls

    CN113263059A

  • Multi-rack working roll shifting method for eliminating local high points of plate strip

    CN114798756A

  • Variable-convexity working roll bending and channeling cooperative control method for local high points of strip steel

    CN116140375A

Cited By

  • Roll shifting method for prolonging rolling period of working rolls of hot-rolled strip steel endless rolling finishing mill group

    CN119608786A

  • Plate strip asymmetric local high point regulation and control method based on rough-finish rolling combined rolling

    CN119870147A

  • Hot rolling working roll bending and shifting cooperative setting method suitable for rolling of various widths

    CN122252467A