A magnetic welding device and its welding method
By adjusting the fiber direction of the magnetized carbon fiber composite material to be consistent with the force direction of the weld joint using magnetic welding equipment, the problems of low welding strength and stability are solved, achieving a high-strength welding effect.
Patent Information
- Application Number
- CN202410756838.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-13
AI Technical Summary
In the prior art, the fiber orientation changes due to heat and pressure during the welding of magnetized carbon fiber composite materials, resulting in low strength and instability of the welded joint.
Magnetically controlled welding equipment is used. The fiber direction is adjusted by a magnetic control device to make it consistent with the force direction of the weld joint. Combined with a pressure output device and current control, precise welding is achieved.
It improves the tensile strength and welding stability of welded joints in the preset stress direction, is suitable for the needs of different welded parts, and enhances the stability and practicality of the welding process.
Smart Images

Figure CN118752784B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite material welding technology, specifically to a magnetically controlled welding device and its welding method. Background Technology
[0002] Carbon fiber composites possess excellent properties such as high specific strength, specific modulus, fatigue resistance, and low coefficient of thermal expansion, and have been widely used in aerospace, weaponry, and transportation fields. Existing technology has successfully prepared magnetized carbon fiber composites, as detailed in patent CN116590913A. The prepared magnetized carbon fiber composites offer advantages such as controllable fiber orientation and high strength, making them a novel type of composite material.
[0003] In existing technologies, resistance welding is generally used when welding magnetized carbon fiber composites. However, the traditional welding method causes the internal fiber orientation of the magnetized carbon fiber composites to change due to heat and pressure during welding, which leads to problems such as low welding strength and unstable welding strength in the welded joint. Summary of the Invention
[0004] To address the problem that welding magnetized carbon fiber composites using traditional resistance welding methods results in low and unstable weld strength in the welded joints, this invention provides a magnetic control welding device.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a magnetically controlled welding device, comprising a main frame, a welding operation platform, a pressure output device, a magnetic control device, and a control device. The welding operation platform is mounted on the main frame; the welding operation platform includes a welding platform and two clamping plates. The welding platform is used to place the workpiece to be welded and to perform welding operations on the workpiece. The two clamping plates are symmetrically mounted on the welding platform and are connected to each other by a heating element. The pressure output device is mounted on the main frame and faces the welding operation platform. The pressure output device includes a cylinder and a pressure head. The pressure head is connected to the cylinder, and the cylinder drives the pressure head to move towards the workpiece placed on the welding platform until it contacts the workpiece and applies pressure to the workpiece. The magnetic control device is mounted on the main frame of the equipment. The magnetic control device includes a ring electromagnet, a mounting bracket for placing the ring electromagnet, and a steering mechanism. The mounting bracket is connected to the steering mechanism, which is adapted to drive the ring electromagnet to rotate via the mounting bracket, so that the direction of the magnetic field generated by the ring electromagnet is consistent with the direction of the force on the workpiece to be welded. The control device includes a welding current control component, a welding pressure control component, and an electromagnetic field strength control component. The two ends of the welding current control component are respectively connected to two clamps, so that the welding current control component, the two clamps, and the heating element form an electrical circuit. The welding pressure control component is electrically connected to the pressure output device to control the output pressure of the welding pressure control component. The electromagnetic field strength control component is electrically connected to the ring electromagnet to control the magnetic field strength of the ring electromagnet.
[0006] A welding method using a magnetic welding device includes the following steps:
[0007] S1, clamp two parts to be welded in a single lap joint, and place one of the parts to be welded on top of the heating element and the other part to be welded below the heating element;
[0008] S2, connect the two ends of the heating element to the two clamps of the magnetic welding equipment respectively, so that the heating element, the two clamps and the welding current control component form an electrical circuit;
[0009] S3, the pressure head in the pressure output device is slowly lowered to press against the welding joint of the two parts to be welded by the welding pressure control component, and then the pressure value is adjusted to the preset pressure value;
[0010] S4. Based on the force direction of the two workpieces to be welded at the welding joint, the magnetic field direction of the annular electromagnet is adjusted through the steering mechanism so that the magnetic field direction of the annular electromagnet is consistent with the force direction of the welding joint; then the current of the electromagnetic field strength control component is adjusted so that the magnetic field strength of the annular electromagnet reaches the preset value.
[0011] S5, start the welding current control component, and then adjust the current value of the welding current control component to the preset value to start the welding operation;
[0012] S6. After welding is completed, first turn off the welding current control component. At this time, the electromagnetic field strength control component and the welding pressure control component continue to work. After the pressure and magnetism are maintained for a period of time, first turn off the electromagnetic field strength control component and then turn off the welding pressure control component.
[0013] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0014] (1) By setting up a magnetic control device, the direction of the internal fibers of the carbon fiber composite material is adjusted during welding, so that the direction of the internal fibers of the carbon fiber composite material can be consistent with the direction of the force of the welded joint during welding. This ensures that the direction of the internal fibers of the welded joint is consistent during welding, thereby improving the tensile strength of the welded joint in its preset force direction and making the welded connection component have high strength characteristics.
[0015] (2) By setting a steering mechanism, the magnetic field direction of the annular electromagnet can be adjusted according to the force direction of different welded joints during welding, so that the magnetic control welding equipment of the present invention can be adjusted according to the force direction of different welded parts during welding, thereby improving the practicality of the entire magnetic control welding equipment and making it suitable for the needs of different welded parts.
[0016] (3) By setting a steering mechanism and cooperating with a gyroscope and a computer control terminal, the angle of the ring electromagnet can be adjusted more precisely so that the direction of the magnetic field generated by the ring electromagnet is consistent with the direction of the force on the weld joint during welding. This allows the fibers in the workpiece to be welded to rotate under the action of the magnetic control device to be consistent with the direction of the force on the weld joint during welding, thereby improving the stability of the welding process and enhancing the tensile strength of the weld joint in the preset force direction after welding. Attached Figure Description
[0017] Figure 1 A schematic diagram of the structure of the magnetic welding equipment provided by the present invention.
[0018] Figure 2 This is a perspective view of the pressure output device, magnetic control device, and welding operation platform installed on the main frame of the equipment in this invention.
[0019] Figure 3 This is a schematic diagram of the magnetic control device and welding operation platform installed on the main frame of the equipment in this invention.
[0020] Figure 4 This is a schematic diagram of the pressure output device and welding operation platform installed on the main frame of the equipment in this invention.
[0021] Figure 5 This is a schematic diagram of the magnetic control device in this invention.
[0022] Figure 6 This is a schematic diagram of the magnetic control device in this invention from another angle.
[0023] Figure 7 This is a schematic diagram of the control device in this invention.
[0024] Figure 8 This is a schematic diagram of another steering mechanism installed on the main frame of the equipment in Embodiment 2 of the present invention.
[0025] Figure 9 This is a circuit diagram showing the connection between the heating element and the clamping plate to form an electrical circuit in Embodiments 4 to 6 of the present invention.
[0026] Figure 10 This is a circuit diagram showing the connection between the heating element and the clamping plate to form an electrical circuit in Embodiments 7 to 9 of the present invention.
[0027] In the diagram: 1. Pressure output device; 11. Cylinder; 12. Pressure head; 2. Main frame of the equipment; 21. Top plate; 22. Side plate; 23. Base plate; 3. Welding operation platform; 31. Welding platform; 32. Clamping plate; 33. Welding support frame; 34. Base; 4. Magnetic control device; 41. Mounting frame one; 42. Support ring one; 421. Support column; 43. Support ring two; 44. Mounting frame two; 45. Drive component one; 46. Drive component two; 47. Rotating handle; 5. Control device 51. Welding pressure control assembly; 511. Control knob; 512. Pressurization knob; 513. Adjustment knob two; 514. Display screen three; 52. Welding current control assembly; 521. Display screen one; 522. Display screen two; 523. Switch one; 524. Adjustment knob one; 53. Electromagnetic field strength control assembly; 531. Display screen four; 532. Display screen five; 533. Switch three; 534. Adjustment knob three; 6. Computer control terminal; 7. Air compressor. Detailed Implementation
[0028] The present invention will now be further described in conjunction with specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.
[0029] In the description of this invention, it should be noted that directional terms such as "center," "lateral," "longitudinal," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation and positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These are used only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. They should not be construed as limiting the specific scope of protection of this invention. The terms "first," "second," etc., in the specification and claims of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. The terms "comprising" and "having," and any variations thereof, in the specification and claims of this invention, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or device that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products, or devices.
[0030] Example 1
[0031] Reference Figure 1As shown, an embodiment of the present invention provides a magnetic control welding device, including a main frame 2, a welding operation platform 3, a pressure output device 1, a magnetic control device 4, a control device 5, and a computer control terminal 6. The welding operation platform 3, pressure output device 1, and magnetic control device 4 are all mounted on the main frame 2. The computer control terminal 6 is connected to the control device 5 and the magnetic control device 4, respectively, and the computer can acquire and store data from the control device 5. The computer control terminal 6 can also control the rotation of the magnetic control device 4 by controlling a steering mechanism. In this embodiment, the main frame 2 includes a top plate 21, a bottom plate 23, and two side plates 22. One end of each side plate 22 is connected to the top plate 21, and the other end is connected to the bottom plate 23. The welding operation platform 3 is mounted on the bottom plate 23, and the magnetic control device 4 is sleeved on the outside of the welding operation platform 3. The bottom of the magnetic control device 4 is fixed to the bottom plate 23, and both sides of the magnetic control device 4 are fixed to the side plates 22 by welding. The magnetic control device 4 provides a uniformly oriented magnetic field to the welding area of the welding platform 3, thereby ensuring consistent fiber orientation in the workpieces to be welded within the welding area and improving the tensile strength of the welded joint in the preset stress direction. Here, the preset stress direction refers to the stress direction of the welded joint during use. The pressure output device 1 is fixedly installed on the top plate 21 and is adapted to provide pressure to the welding platform 3.
[0032] In this embodiment, the workpiece to be welded can be magnetic carbon fiber reinforced nylon VI, which contains magnetic carbon fibers. The heating element is a component with resistance heating effect, such as stainless steel wire mesh.
[0033] The dimensions of each part to be welded should not exceed 160mm*60mm, the thickness should be in the range of 2 to 5mm, and the diameter of the magnetized fiber in the part to be welded should be in the range of 3 to 6μm.
[0034] Please see Figures 2 to 4 The welding operation platform 3 includes a welding platform 31 and two clamping plates 32. The welding platform 31 is used to place two workpieces to be welded and to perform welding operations at the joint of the two workpieces. The two clamping plates 32 are symmetrically mounted on the welding platform 31 and are connected by a heating element. The two workpieces to be welded are located on both sides of the heating element, allowing the heating element to perform resistance welding at the joint of the two workpieces. The clamping plates 32 are brass clamps, each with a double-layer structure. The double-layer structure of the clamping plates 32 clamps the heating element, thereby connecting the two clamping plates 32 through the heating element to form an electrical circuit. In this embodiment, the clamping plates can be brass clamps, and the clamping pressure of the brass clamps can be adjusted between 4MPa and 20MPa.
[0035] Please see Figures 2 to 4The pressure output device 1 includes a cylinder 11, a pressure head 12, and an air compressor 7. The air compressor 7 is connected to the cylinder 11 via an air pipe to supply gas to the cylinder 11. The other end of the cylinder 11 is connected to the pressure head 12, allowing the cylinder 11 to move the pressure head 12 towards the workpiece placed on the welding platform 31 until it contacts the workpiece and applies pressure. The cylinder 11 can be connected to a welding pressure control assembly 51 via an air pipe, allowing the welding pressure control assembly 51 to control the pressure of the cylinder 11. Before welding begins, the welding pressure control assembly 51 changes the pressure of the cylinder 11, and the pressure is transmitted to the surface of the workpiece through the pressure head 12. The pressure output range of the cylinder 11 is 0.2 MPa to 0.6 MPa.
[0036] Please see Figure 5 and Figure 6 The magnetic control device 4 includes a ring electromagnet, a mounting bracket 41 for holding the ring electromagnet, and a steering mechanism. The ring electromagnet is adapted to generate a magnetic field after being energized. The mounting bracket 41 is connected to the steering mechanism, which is adapted to drive the ring electromagnet to rotate through the mounting bracket 41, so that the direction of the magnetic field generated by the ring electromagnet is consistent with the direction of force on the workpiece during welding. In this invention, because ordinary resistance welding causes the fiber direction inside the magnetic carbon fiber reinforced nylon 6 to change, the welding strength of the weld joint in its direction of force is unstable during welding. However, by setting the magnetic control device 4, this invention can provide a uniformly oriented magnetic field in the welding area during welding, so that the fiber direction inside the workpiece is consistent with the direction of force on the weld joint during welding, thus giving the welded joint the advantage of high strength.
[0037] In this embodiment, the wires of the ring electromagnet are connected to the electromagnetic field strength control component 53. The electromagnetic field strength control component 53 is adapted to display the current and voltage generated by the ring electromagnet. Before welding begins, the magnetic control device 4 is controlled by the computer control terminal 6 to rotate the ring electromagnet to a preset angle. This preset angle needs to be determined based on the direction of force on the weld joint during welding. The preset angle of the ring electromagnet needs to be consistent with the direction of force on the weld joint during welding.
[0038] The direction of force on the welded joint can be measured using angle measuring instruments such as angle meters. In this embodiment, the rotation angle of the ring electromagnet can be controlled by a computer control terminal 6 and a gyroscope. The gyroscope can be mounted on the mounting bracket 41 and rotates coaxially with the ring electromagnet, allowing the gyroscope to monitor the rotation angle of the ring electromagnet in real time. Therefore, in actual operation, a preset angle can be input to the computer control terminal 6, and then the computer control terminal 6 and the gyroscope can work together to make the ring electromagnet rotate to the preset angle. This application uses a gyroscope to precisely control the rotation angle of the ring electromagnet, ensuring that the ring electromagnet rotates accurately until the magnetic field direction is consistent with the direction of force on the welded joint during welding. Furthermore, when the magnetic control device 4 rotates, the ring electromagnet is de-energized, preventing the magnetic field generated by the ring electromagnet from affecting the gyroscope.
[0039] To ensure that there is no interference between the various devices, the rotation angle of the magnetic control device 4 in the vertical direction should be between -80° and 80° in this invention, and the cylinder 11 will not move up and down when the magnetic control device 4 is rotating.
[0040] Please see Figure 7 The control device 5 includes a welding current control component 52, a welding pressure control component 51, and an electromagnetic field strength control component 53.
[0041] The welding current control component 52 is connected to two clamping plates 32 at its two ends, forming an electrical circuit with the welding current control component 52, the two clamping plates 32, and the heating element. Resistance welding can be performed by placing the welding joints of the two workpieces to be welded onto the heating element. During welding, the welding current can be adjusted throughout the welding process using the welding current control component 52. In this embodiment, the current adjustment range of the welding current control component 52 is 0-30A.
[0042] The welding pressure control component 51 is electrically connected to the pressure output device 1 and is used to control the output pressure of the welding pressure control component 51. Specifically, the welding pressure control component 51 is connected to the air compressor 7, which allows control of the output pressure of the cylinder 11 by controlling the amount and speed of gas supplied by the air compressor 7 to the cylinder 11. Before welding begins, the pressure of the cylinder 11 can be changed by the welding pressure control component 51, and the pressure is transmitted to the welding joint surface of the two workpieces to be welded through the pressure head 12. In this embodiment, the adjustable pressure range of the welding pressure control component 51 is 0 to 0.6 MPa.
[0043] During the welding process, the pressure output device 1 always provides uniform pressure, which ensures uniform resin flow at the welding interface and further improves the welding strength of the welded joint after welding.
[0044] The electromagnetic field strength control component 53 is electrically connected to the ring electromagnet and is used to control the magnetic field strength of the ring electromagnet. Throughout the welding process, the electromagnetic field strength generated by the ring electromagnet should be within the range of 60mT to 180mT.
[0045] Please see Figure 3 The distance from the welding platform 31 to the bottom of the main frame 2 of the equipment is equal to the distance from the annular electromagnet to the bottom of the main frame 2 of the equipment, and the center of the annular electromagnet coincides with the center point of the welding platform 31. Through the above settings, the annular electromagnet can provide a uniformly oriented magnetic field to the welding joint on the welding platform 31, thereby ensuring that the fiber direction in the workpiece is consistent and improving the strength of the welded joint after welding.
[0046] Please see Figure 4 The welding operation platform 3 also includes a welding support frame 33 and a base 34. One end of the welding support frame 33 is connected to the welding platform 31, and the other end of the welding support frame 33 is connected to the base 34. The base 34 is fixedly installed on the main frame 2 of the equipment. The welding operation platform 3 can be installed on the base plate 23 by drilling holes in the base 34.
[0047] Please see Figure 5 and Figure 6 The steering mechanism includes a first support ring 42, a second support ring 43, two mounting brackets 44, a first drive component 45, and a second drive component 46. The first support ring 42 has multiple support columns 421, which are fixedly mounted on the main frame 2 of the equipment. During actual installation, the magnetic control device 4 can be fixed by fixing the support columns 421 to the base plate 23. The outer diameter of the second support ring 43 is smaller than the inner diameter of the first support ring 42. The second support ring 43 is slidably mounted on the inner side of the first support ring 42. This sliding mounting improves the stability of the second support ring 43 when it rotates due to the first drive component 45. The first drive component 45 connects to the second support ring 43, allowing it to rotate the second support ring 43 along the axial direction (i.e., horizontal direction) of the first support ring 42, thereby adjusting the positional relationship between the annular electromagnet and the workpiece to be welded on the welding platform 31 in the horizontal direction. Two mounting brackets 44 are symmetrically mounted on the support ring 43. The two ends of mounting bracket 41 are rotatably mounted on the two mounting brackets 44. A driving component 46 is connected to mounting bracket 41, allowing it to rotate along the radial direction of the support ring 42. By controlling the driving component 46, the positional relationship between the annular electromagnet and the workpiece to be welded on the welding platform 31 in the vertical direction can be controlled. In this embodiment, by setting the driving component 45 and the driving component 46, the position of the annular electromagnet can be effectively adjusted, allowing it to rotate relatively precisely to a position where the direction of the generated magnetic field is consistent with the direction of the force experienced by the weld joint during welding.
[0048] It is understood that in order to improve the welding strength of the welded joint in the direction of force, this embodiment generates a magnetic field by setting a magnetic control device 4. Under the action of the magnetic field, the direction of most of the fibers in the magnetic carbon fiber is consistent with the direction of force of the welded joint during welding, thereby improving the welding strength of the welded joint in the preset direction of force.
[0049] In this embodiment, in order to further enhance the stability of the magnetic control device 4 installed on the main frame 2 of the equipment, the part of the outer wall of the support ring 42 facing the side plate 22 can be directly welded to the side plate 22, thereby further improving the stability of the fixation between the magnetic control device 4 and the main frame 2 of the equipment, and also improving the stability of the steering mechanism when it drives the ring electromagnet to rotate.
[0050] In this embodiment, drive component 1 45 and drive component 2 46 can be motors.
[0051] The inner side of the support ring 42 may be provided with a gear 1, and the output shaft of the drive member 45 is provided with a gear 2 that meshes with the gear 1. Under the mutual meshing of the gear 1 and the gear 2, the support ring 42 can be rotated by the drive member 45.
[0052] Among them, the second driving component 46 is fixedly installed on the second mounting bracket 44. The second driving component 46 is connected to the first mounting bracket 41 through gear meshing, so that the second driving component 46 can drive the first mounting bracket 41 to rotate through the gear.
[0053] In this embodiment, drive component 45 and drive component 46 can be motors.
[0054] The control device 5 is also equipped with a power supply, which is connected to the welding current control component 52, the welding pressure control component 51 and the electromagnetic field strength control component 53 respectively, so as to supply power to the welding current control component 52, the welding pressure control component 51 and the electromagnetic field strength control component 53 respectively.
[0055] like Figure 7As shown, the welding current control component 52 includes a first display screen 521, a second display screen 522, an adjustment knob 524, and a first switch 523. The first display screen 521, the second display screen 522, the adjustment knob 524, and the first switch 523 are all mounted on the control panel of the control device 5. The first display screen 521 is suitable for displaying real-time data of the welding voltage during the welding process, and the second display screen 522 is suitable for displaying real-time data of the welding current during the welding process. During the actual welding process, the current and voltage during the welding process can be observed in real time through the first display screen 521 and the second display screen 522. Simultaneously, the welding current control component 52 can also be connected to the computer control terminal 6 to transmit data such as the current and voltage during the welding process to the computer control terminal 6 for storage. The adjustment knob 524 is used to adjust the current value during the welding process, and the first switch 523 is suitable for controlling the opening or closing of the entire welding current control component 52. Before welding begins, the first switch 523 needs to be turned on to activate the welding current control component 52, enabling it to supply power to the heating element, thereby achieving the purpose of resistance welding. The current value during welding can also be adjusted by adjusting knob 524.
[0056] like Figure 7 As shown, the welding pressure control assembly 51 includes a display screen 514, a control knob 511, a pressure knob 512, an adjustment knob 513, and a switch. The display screen 514, control knob 511, pressure knob 512, adjustment knob 513, and switch 513 are all mounted on the control panel of the control device 5. The display screen 514 is used to display the preset pressure value of the pressure output device 1 during welding. The control knob 511 is used to control the cylinder 11 to move the pressure head 12 toward or away from the welding platform 31. The pressure knob 512 is used to adjust the pressure of the pressure output device 1 to the preset pressure value displayed on the display screen 514. The adjustment knob 513 is used to adjust the preset pressure value displayed on the display screen 514. The switch 513 is used to control the opening or closing of the entire welding pressure control assembly 51.
[0057] like Figure 7As shown, the electromagnetic field strength control component 53 includes a fourth display screen 531, a fifth display screen 532, an adjustment knob 534, and a third switch 533. The fourth display screen 531, the fifth display screen 532, the adjustment knob 534, and the third switch 533 are all mounted on the control panel of the control device 5. The fourth display screen 531 is suitable for displaying the real-time voltage of the magnetic field generated by the ring electromagnet, and the fifth display screen 532 is suitable for displaying the real-time current of the magnetic field generated by the ring electromagnet. The magnetic field strength generated by the ring electromagnet can be calculated from the current, and the force on the workpiece to be welded in the magnetic field can be calculated by combining the voltage. For the specific calculation process, refer to Embodiment 3. The adjustment knob 534 is used to adjust the current value displayed on the fifth display screen 532, and the second switch is suitable for controlling the opening or closing of the entire electromagnetic field strength control component 53.
[0058] Example 2
[0059] like Figure 8 As shown, this embodiment provides a magnetic welding device, whose structure is basically the same as that of Embodiment 1, except that the steering mechanism in Embodiment 2 is a rotating handle 47. In this embodiment, both ends of the mounting bracket 41 are rotatably mounted on the side plates 22 of the main frame 2 of the equipment, and the rotating handle 47 is fixedly mounted on one side of the mounting bracket 41. In actual operation, the rotating handle 47 can be rotated to drive the annular electromagnet placed in the mounting bracket 41 to rotate, which can effectively adjust the position of the annular electromagnet so that it can be rotated more accurately to a position where the direction of the generated magnetic field is consistent with the direction of the force on the welding joint during welding.
[0060] Example 3
[0061] A welding method using a magnetic welding device includes the following steps:
[0062] S1, clamp two parts to be welded in a single lap joint and place them on both sides of the heating element;
[0063] S2, connect the two ends of the heating element to the two clips respectively, so that the heating element, the two clips and the welding current control assembly form an electrical circuit;
[0064] S3, the pressure head in the pressure output device is slowly lowered to press against the welding joint of the two parts to be welded by the welding pressure control component, and then the pressure of the pressure output device is adjusted to the preset pressure value;
[0065] S4. According to the force direction of the welded joint, the magnetic field direction of the ring electromagnet is adjusted by the steering mechanism so that the magnetic field direction of the ring electromagnet is consistent with the force direction of the workpiece to be welded; then the current of the electromagnetic field strength control component is adjusted so that the magnetic field strength of the ring electromagnet reaches the preset value.
[0066] S5, start the welding current control component, and then adjust the current value of the welding current control component to the preset value to start the welding operation;
[0067] S6. After welding is completed, first turn off the welding current control component. At this time, the electromagnetic field strength control component and the welding pressure control component continue to work. After the pressure and magnetism are maintained for a period of time, turn off the electromagnetic field strength control component first and then turn off the welding pressure control component.
[0068] The formula for calculating the temperature of the heating element during welding is as follows:
[0069]
[0070] In the formula, T He The heating element temperature is represented by I, the current magnitude by R, the resistance of the heating element by A, and the heat dissipation area by T. r The value represents room temperature, and η1 represents heat dissipation efficiency, η1 = 20~30 W / (m·K);
[0071] The formula for calculating welding time during the welding process is:
[0072] t H =2Q / KL 搭
[0073] Among them, t H Where is the welding time, Q is the specific heat capacity of the workpiece to be welded, K is the thermal conductivity of the workpiece to be welded, and L is the welding time. 搭 This refers to the overlap distance of the workpieces to be welded along the direction of the heating element.
[0074] Welding pressure is inversely proportional to the porosity of the heating element and inversely proportional to the temperature of the workpiece. The empirical formula for calculating welding pressure is as follows:
[0075]
[0076] Where P is the welding pressure and ζ is an empirical coefficient. T represents the porosity of the heating element. He The temperature of the heating element;
[0077] The formula for calculating the magnetic field strength of a ring electromagnet is:
[0078] H = N × I / L
[0079] Where H is the magnetic field strength of the ring electromagnet, with units of A / m, N is the number of turns of the coil, I is the current flowing through the coil, and L is the length of the coil;
[0080] The formula for the magnitude of the force on the workpiece in the magnetic field is:
[0081] F 磁 =m*x*V*H
[0082] Where m is the mass of the part to be welded, x is the specific magnetization coefficient of the magnetic fiber, and the calculation formula is k*ρ, where k is the volume magnetic susceptibility, ρ is the density, V is the volume of the magnetic fiber, and H is the magnetic field strength of the ring electromagnet.
[0083] The formula for the magnitude of the torque experienced by the workpiece in a magnetic field is:
[0084] M = F 磁 *0.25L 纤维
[0085] Where M is the magnitude of the torque experienced by the magnetic fiber in the magnetic field, and L 纤维 F represents the length of the fiber. 磁 This represents the magnitude of the force exerted on the magnetic fiber in the magnetic field.
[0086] The formula for calculating the holding time after welding is as follows:
[0087]
[0088] Where t represents the holding time, I represents the current value in the welding pressure control component, R represents the resistance value of the heating element, and T He T represents the temperature of the heating element. r Let A represent the room temperature, A represent the heat dissipation area, and t represent the heat dissipation area. H The welding time is indicated by η1, which represents the heat dissipation efficiency of the heating element through the workpiece to be welded to the air. η1 = 5~10 W / (m·K); η2 represents the heat dissipation efficiency of the welded joint. η2 = 18~25 W / (m·K).
[0089] In this embodiment, the heating element is a stainless steel mesh, which needs to be pre-treated before welding. The pre-treatment includes the following steps: (1) Use 100# sandpaper to polish both sides of the mesh 10 to 20 times.
[0090] (2) Immerse the metal mesh in a mixed solution at 40-60℃ for 5-10 minutes. The mixed solution consists of 40-45 g / L NaOH and 5-10 g / L Na2CO3.
[0091] (3) Place the soaked metal mesh into anhydrous ethanol and ultrasonically clean it for 5 to 10 minutes at 100 to 120 W and 40 to 50 kHz.
[0092] (4) Place the ultrasonically cleaned metal mesh into HCl at 25-35℃ and 10-15% for 1-2 minutes for acid washing.
[0093] (5) Wash the stainless steel mesh with deionized water and dry it with a hair dryer.
[0094] Example 4
[0095] A magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding component. The dimensions of the magnetic fiber composite material sheet were 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type was T300, and the matrix was polycaprolactam (PA6). The heating element was a metal mesh with dimensions of 100mm in length × 20mm in width. The metal mesh type was 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0096] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0097] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =250℃.
[0098] Calculate the specific heat capacity of the workpiece to be welded:
[0099]
[0100] Calculate the welding current;
[0101] I = [(T He -T r )η1A / R] 1 / 2 =[(250℃-20℃)×25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =6.3A
[0102] Calculate welding time:
[0103] t H =2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0104] Calculate welding pressure:
[0105] For the material in this example, the empirical coefficient ζ = 36.4
[0106]
[0107] Calculation range of magnetic field strength:
[0108] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0109] Calculate the pressure holding and magnetization holding time:
[0110]
[0111] Considering the differences in actual heat dissipation performance, and to ensure that the connector temperature cools to room temperature, we take t = 300s.
[0112] The wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve surface roughness. Both sides of the wire mesh are sanded 15 times with 100# sandpaper. The wire mesh is then immersed in a mixed solution at 60℃ for 8 minutes to remove surface impurities. The mixed solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the wire mesh is ultrasonically cleaned in anhydrous ethanol at 100 W and 50 kHz for 10 minutes. Following ultrasonic cleaning, the wire mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the wire mesh is washed with deionized water for 1 minute. After washing, it is dried with a hairdryer.
[0113] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0114] The base materials (i.e., the two parts to be welded) are placed on the welding platform in an overlapping manner, with an overlap length L. 搭 The overlap width is 20mm, and the overlap joint is placed below the pressure head. Place the metal mesh inside the overlap joint, and connect clips to both ends of the metal mesh, as shown. Figure 9 As shown.
[0115] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head at a low pressure until it presses against the weld joint of the two parts to be welded. After the pressure head presses against the weld joint, turn the pressure knob to increase the cylinder pressure to 0.38 MPa.
[0116] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the annular electromagnet to make it 80° with the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0117] Turn on switch one to start the welding operation. Turn on adjustment knob one to adjust the welding current to 6.3A. Set the welding time to 35 seconds.
[0118] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 300 seconds. Then, first turn off the electromagnetic field strength control component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0119] The welded joint prepared in Example 4 was verified by tensile testing. The dimensions of the tensile specimen were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. A standard tensile specimen and a backing plate of the same thickness as the specimen were prepared. When mounting the specimen on the tensile testing machine, the backing plate was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 20.52 MPa.
[0120] Example 5
[0121] Magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding base material. The dimensions of the magnetic fiber composite material plate are 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type is T300, and the matrix is polycaprolactam (PA6). The metal mesh size is 100mm in length × 20mm in width. The metal mesh type is 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0122] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0123] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =320℃.
[0124] Calculate the specific heat capacity of magnetic fiber reinforced materials:
[0125]
[0126] Calculate the welding current;
[0127] I = [(T He -T r )η1A / R] 1 / 2 =[(320℃-20℃)×25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =7.1A
[0128] Calculate welding time:
[0129] t H =2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0130] Calculate welding pressure:
[0131] For the material in this example, the empirical coefficient ζ = 36.4
[0132]
[0133] Calculation range of magnetic field strength:
[0134] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0135] Calculate the pressure holding and magnetization holding time:
[0136]
[0137] Considering the differences in actual heat dissipation performance, and to ensure that the connector temperature cools to room temperature, we take t = 300s.
[0138] The metal wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve its surface roughness. Both sides of the metal mesh are sanded 15 times using 100# sandpaper. The metal mesh is then immersed in a mixed solution at 60℃ for 8 minutes. This solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the metal mesh is placed in anhydrous ethanol and ultrasonically cleaned for 10 minutes at 100 W and 50 kHz. Following this, the ultrasonically cleaned metal mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the metal mesh is rinsed with deionized water for 1 minute. After washing, it is dried with a hair dryer.
[0139] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0140] Place the two base materials (i.e., the two parts to be welded) on the welding platform in an overlapping manner, with an overlap length of 20mm and an overlap width of 20mm. The overlap joint is placed under the pressure head. Place the metal mesh inside the overlap joint, and connect clamps to both ends of the metal mesh.
[0141] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head to the weld joint at a low pressure. After the pressure head reaches the weld joint, turn the pressure knob to increase the cylinder pressure to 0.3 MPa.
[0142] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the annular electromagnet to make it 80° with the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0143] Turn on switch one to start the welding operation. Turn the adjustment knob one to adjust the welding current to 7.1A. Set the welding time to 35s.
[0144] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 300 seconds. Then, first turn off the electromagnetic field strength controller component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0145] The welded joint prepared in Example 5 was verified by tensile testing. The dimensions of the tensile specimen were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. A standard tensile specimen and a backing plate of the same thickness as the specimen were prepared. When mounting the specimen on the tensile testing machine, the backing plate was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 22.55 MPa.
[0146] Example 6
[0147] Magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding base material. The dimensions of the magnetic fiber composite material plate are 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type is T300, and the matrix is polycaprolactam (PA6). The metal mesh size is 100mm in length × 20mm in width. The metal mesh type is 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0148] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0149] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =380℃.
[0150] Calculate the specific heat capacity of magnetic fiber reinforced materials:
[0151]
[0152] Calculate the welding current;
[0153] I = [(T He -T r )η1A / R] 1 / 2 =[(380℃-20℃)×25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =9.4A
[0154] Calculate welding time:
[0155] t H =2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0156] Calculate welding pressure:
[0157] For the material in this example, the empirical coefficient ζ = 36.4
[0158]
[0159] Calculation range of magnetic field strength:
[0160] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0161] Calculate the pressure holding and magnetization holding time:
[0162]
[0163] Considering the differences in actual heat dissipation performance, and to ensure that the connector temperature cools to room temperature, we take t = 350s.
[0164] The metal wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve its surface roughness. Both sides of the metal mesh are sanded 15 times using 100# sandpaper. The metal mesh is then immersed in a mixed solution at 60℃ for 8 minutes. This solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the metal mesh is placed in anhydrous ethanol and ultrasonically cleaned for 10 minutes at 100 W and 50 kHz. Following this, the ultrasonically cleaned metal mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the metal mesh is rinsed with deionized water for 1 minute. After washing, it is dried with a hair dryer.
[0165] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0166] The base material is placed on the welding platform in an overlapping manner, with an overlap length of 20mm and an overlap width of 20mm. The overlapping joint is placed below the pressure head. A metal mesh is placed inside the overlapping joint, and clips are connected to both ends of the metal mesh.
[0167] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head to the weld joint at a low pressure. After the pressure head reaches the weld joint, turn the pressure knob to increase the cylinder pressure to 0.25 MPa.
[0168] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the annular electromagnet to make it 80° with the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0169] Turn on switch one to start the welding operation. Turn the adjustment knob one to adjust the welding current to 9.4A. Set the welding time to 35 seconds.
[0170] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 350 seconds. Then, first turn off the electromagnetic field strength control component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0171] The welded joint prepared in Example 6 was verified by tensile testing. The dimensions of the tensile specimen were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. A standard tensile specimen and a backing plate of the same thickness as the specimen were prepared. When mounting the specimen on the tensile testing machine, the backing plate was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 22.70 MPa.
[0172] The mechanical properties of the magnetic short-cut carbon fiber oriented reinforced PA6 welded joints prepared in Examples 4 to 6 were compared with those of the prior art PA6 welded joints without magnetic short-cut carbon fiber oriented reinforcement under the same welding parameters and the same load mode. The results are shown in Table 1 below.
[0173]
[0174] As shown in Table 1, the welded joints prepared from magnetized carbon fiber composite materials in each of Examples 4 to 6 exhibit significantly greater strength in the predetermined stress direction than the welded joints prepared from unmagnetized carbon fiber composite materials. This demonstrates that the present invention, by orienting the fibers within the carbon fiber composite material using a magnetic control device, can effectively enhance the strength of the welded joint in the predetermined stress direction, thus ensuring that the carbon fiber composite material maintains its high strength during welding.
[0175] Example 7
[0176] Magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding base material. The dimensions of the magnetic fiber composite material plate are 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type is T300, and the matrix is polycaprolactam (PA6). The metal mesh size is 100mm in length × 20mm in width. The metal mesh type is 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0177] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0178] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =380℃.
[0179] Calculate the specific heat capacity of magnetic fiber reinforced materials:
[0180]
[0181] Calculate the welding current;
[0182] I = [(T He -T r )η1A / R]1 / 2 =[(380℃-20℃)25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =9.4A
[0183] Calculate welding time:
[0184] t=2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0185] Calculate welding pressure:
[0186] For the material in this example, the empirical coefficient ζ = 36.4
[0187]
[0188] Calculation range of magnetic field strength:
[0189] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0190] Calculate the pressure holding and magnetization holding time:
[0191]
[0192] Considering differences in actual heat dissipation performance, to ensure the connector temperature cools to room temperature, t is taken as... k =350s.
[0193] The metal wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve its surface roughness. Both sides of the metal mesh are sanded 15 times using 100# sandpaper. The metal mesh is then immersed in a mixed solution at 60℃ for 8 minutes. This solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the metal mesh is placed in anhydrous ethanol and ultrasonically cleaned for 10 minutes at 100 W and 50 kHz. Following this, the ultrasonically cleaned metal mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the metal mesh is rinsed with deionized water for 1 minute. After washing, it is dried with a hair dryer.
[0194] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0195] The base material is placed on the welding platform in an overlapping manner, with an overlap length of 20mm and an overlap width of 20mm. The overlapping joint is placed on the pressure head.
[0196] Below. Place the metal mesh inside the lap joint. Connect clips to both ends of the metal mesh.
[0197] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head to the weld joint at a low pressure. After the pressure head reaches the weld joint, turn the pressure knob to increase the cylinder pressure to 0.25 MPa.
[0198] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the ring electromagnet to make it parallel to the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0199] Turn on switch one to start the welding operation. Turn the adjustment knob one to adjust the welding current to 9.4A. Set the welding time to 35 seconds.
[0200] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 350 seconds. Then, first turn off the electromagnetic field strength control component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0201] The welded joint prepared in Example 7 was verified by tensile testing. The dimensions of the tensile specimens were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. When mounting the specimens on the tensile testing machine, a pad was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 7.43 MPa.
[0202] Example 8
[0203] A magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding base material. The dimensions of the magnetic fiber composite material sheet were 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type was T300, and the matrix was polycaprolactam (PA6). A magnetic fiber reinforced film with a mixed carbon fiber content of 60% (the ratio of magnetized fiber to unmagnetized fiber was 1:1) was selected. The film matrix was the same as the welding base material, which was polycaprolactam (PA6). The dimensions of the metal mesh were 100mm in length × 20mm in width. The metal mesh type was 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0204] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0205] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =380℃.
[0206] Calculate the specific heat capacity of magnetic fiber reinforced materials:
[0207]
[0208] Calculate the welding current;
[0209] I = [(T He -T r )η1A / R] 1 / 2 =[(380℃-20℃)25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =9.4A
[0210] Calculate welding time:
[0211] t H =2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0212] Calculate welding pressure:
[0213] For the material in this example, the empirical coefficient ζ = 36.4
[0214]
[0215] Calculation range of magnetic field strength:
[0216] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0217] Calculate the pressure holding and magnetization holding time:
[0218]
[0219] Considering the differences in actual heat dissipation performance, and to ensure that the connector temperature cools to room temperature, we take t = 350s.
[0220] The metal wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve its surface roughness. Both sides of the metal mesh are sanded 15 times using 100# sandpaper. The metal mesh is then immersed in a mixed solution at 60℃ for 8 minutes. This solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the metal mesh is placed in anhydrous ethanol and ultrasonically cleaned for 10 minutes at 100 W and 50 kHz. Following this, the ultrasonically cleaned metal mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the metal mesh is rinsed with deionized water for 1 minute. After washing, it is dried with a hair dryer.
[0221] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0222] The base material is placed on the welding platform in an overlapping manner, with an overlap length of 20mm and an overlap width of 20mm. The overlapping joint is placed below the pressure head. The metal mesh and the mixed fiber-reinforced film are placed inside the overlapping joint. Clips are connected to both ends of the metal mesh. The overlapping joint is placed in the following order from bottom to top: fiber-reinforced plate, fiber-reinforced film, heating element, fiber-reinforced film, fiber-reinforced plate. Figure 10 As shown.
[0223] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head to the weld joint at a low pressure. After the pressure head reaches the weld joint, turn the pressure knob to increase the cylinder pressure to 0.25 MPa.
[0224] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the annular electromagnet to make it 80° with the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0225] Turn on switch one to start the welding operation. Turn the adjustment knob one to adjust the welding current to 9.4A. Set the welding time to 35 seconds.
[0226] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 350 seconds. Then, first turn off the electromagnetic field strength controller component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0227] The welded joint prepared in Example 8 was verified by tensile testing. The dimensions of the tensile specimens were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. When mounting the specimens on the tensile testing machine, a pad was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 23.90 MPa.
[0228] Example 9
[0229] A magnetic fiber composite material with a magnetic carbon fiber content of 30% was selected as the welding base material. The dimensions of the magnetic fiber composite material sheet were 50mm in length × 20mm in width × 3mm in thickness. The carbon fiber type was T300, and the matrix was polycaprolactam (PA6). A magnetic fiber reinforced film with a mixed carbon fiber content of 60% (the ratio of magnetized fiber to unmagnetized fiber was 1:1) was selected. The film matrix was the same as the welding base material, which was polycaprolactam (PA6). The dimensions of the metal mesh were 100mm in length × 20mm in width. The metal mesh type was 200 mesh, with a wire diameter of 0.05mm, a pore size of 0.08mm, and a porosity of 37.9%.
[0230] The specific magnetic susceptibility of the magnetized fiber is x = 5.27 emu / kg.
[0231] Heating element temperature range: 220℃ < T He <580℃, this example selects T He =380℃.
[0232] Calculate the specific heat capacity of magnetic fiber reinforced materials:
[0233]
[0234] Calculate the welding current;
[0235] I = [(T He -T r )η1A / R] 1 / 2 =[(380℃-20℃)25W / (m·K)×5×10 -3 m 2 / 0.5Ω] 1 / 2 =9.4A
[0236] Calculate welding time:
[0237] t H =2Q / KL 搭 =[2×1.19J / (kg·K)] / (3.4×0.02m)=35s
[0238] Calculate welding pressure:
[0239] For the material in this example, the empirical coefficient ζ = 36.4
[0240]
[0241] Calculation range of magnetic field strength:
[0242] g / 2xV<H<g / xV; that is, 3A / m<H<6A / m
[0243] Calculate the pressure holding and magnetization holding time:
[0244]
[0245] Considering the differences in actual heat dissipation performance, and to ensure that the connector temperature cools to room temperature, we take t = 350s.
[0246] The metal wire mesh undergoes pre-welding treatment to remove oxides, grease, and other impurities from its surface and to improve its surface roughness. Both sides of the metal mesh are sanded 15 times using 100# sandpaper. The metal mesh is then immersed in a mixed solution at 60℃ for 8 minutes. This solution consists of 40 g / L NaOH and 10 g / L Na₂CO₃. After immersion, the metal mesh is placed in anhydrous ethanol and ultrasonically cleaned for 10 minutes at 100 W and 50 kHz. Following this, the ultrasonically cleaned metal mesh is acid-washed in 15% HCl at 25℃ for 1 minute. Finally, the metal mesh is rinsed with deionized water for 1 minute. After washing, it is dried with a hair dryer.
[0247] Before welding, the magnetic fiber composite material is treated by wiping the surface of the material three times with acetone and then letting it dry.
[0248] The base material is placed on the welding platform in an overlapping manner, with an overlap length of 20mm and an overlap width of 20mm. The overlapping joint is placed below the pressure head. The metal mesh and the mixed fiber reinforced film are placed inside the overlapping joint. Clips are connected to both ends of the metal mesh. The overlapping joint is placed in the following order from bottom to top: fiber reinforced plate, fiber reinforced film, heating element, fiber reinforced film, fiber reinforced plate.
[0249] Before welding, turn the control knob, and the cylinder will slowly lower the pressure head to the weld joint at a low pressure. After the pressure head reaches the weld joint, turn the pressure knob to increase the cylinder pressure to 0.25 MPa.
[0250] After the cylinder descends and is pressurized, the computer-controlled magnetic control device rotates the ring electromagnet to make it parallel to the ground, switches three are turned on, and adjustment knob three is rotated until the magnetic field strength is 5A / m.
[0251] Turn on switch one to start the welding operation. Turn the adjustment knob one to adjust the welding current to 9.4A. Set the welding time to 35 seconds.
[0252] After the set welding time is reached, turn off the welding current control component and maintain the electromagnetic field strength and welding pressure constant for 350 seconds. Then, first turn off the electromagnetic field strength control component, and then turn off the pressure knob and control knob of the welding pressure control component in sequence.
[0253] The welded joint prepared in Example 9 was verified by tensile testing. The dimensions of the tensile specimens were in accordance with the requirements of GB / T3335—2014 and ASTM D5868-01. When mounting the specimens on the tensile testing machine, a pad was used to compensate for the lap offset. The tensile strength of the welded joint was measured to be 9.76 MPa.
[0254] Among them, the fiber-reinforced films in Examples 7 to 9 can be divided into three types: unmagnetized fiber-reinforced films, magnetized fiber-reinforced films, and mixed fiber-reinforced films (a mixture of unmagnetized and magnetized fibers). Different fiber-reinforced films can be selected to meet the requirements of different welding base materials and the mechanical properties of the weld joint.
[0255] For base materials that are unmagnetized fiber composites, magnetized fiber reinforced films or hybrid fiber reinforced films can be used to introduce magnetized fibers at the joint. During the welding process, the magnetic field controls the rotation of the magnetized fibers to a preset direction, thereby enhancing the mechanical properties of the unmagnetized fiber composite welded joint in the preset direction.
[0256] For base materials that are magnetized fiber composites, unmagnetized fiber reinforced films or mixed fiber reinforced films can be used to introduce unmagnetized fibers at the joint. During the welding process, the magnetic field controls the original magnetized fibers of the base material to rotate to a preset direction, while the unmagnetized fibers introduced through the unmagnetized fiber reinforced film are not controlled by the magnetic field and their fiber directions are randomly distributed, thereby enhancing the external mechanical properties of the welded joint in the preset direction.
[0257] To enhance mechanical properties in a predetermined direction, a magnetized fiber reinforced film can be used, with magnetized fibers introduced at the joint. During welding, a magnetic field controls the rotation of the magnetized fibers to the predetermined direction, thereby enhancing the shear strength in that direction.
[0258] To enhance the required external mechanical properties in a predetermined direction, a magnetized fiber reinforced film can be used, with magnetized fibers introduced at the joint. During welding, a magnetic field controls the rotation of the magnetized fibers to the predetermined direction, thereby enhancing the shear strength in that direction.
[0259] The mechanical properties of the magnetic short-cut carbon fiber oriented reinforced PA6 welded joints prepared in Examples 6 to 9 under the same welding parameters and the same load were compared in the direction of force. The results are shown in Table 2 below.
[0260]
[0261] As demonstrated in Examples 6 and 8, under the same welding parameters and load conditions, the tensile strength of the welded joint prepared in Example 8 in the predetermined stress direction is significantly greater than that of the welded joint prepared in Example 6. The main reason is the addition of a fiber-reinforced film to the workpiece (i.e., the magnetized carbon fiber composite material). This fiber-reinforced film effectively increases the total number of fibers within the entire welded joint, and under the action of the magnetic control device, more fibers within it are oriented in the same direction as the stress direction during welding, thus further enhancing the strength of the welded joint in the predetermined stress direction.
[0262] As demonstrated by Examples 7 and 9, under the same welding parameters and load conditions, the tensile strength of the welded joint in Example 9, outside the preset stress direction, is greater than that of the welded joint in Example 7. This is primarily because a fiber-reinforced film is added to the workpiece to be welded (i.e., the magnetized carbon fiber composite material). This film effectively increases the total number of fibers within the entire welded joint, and since the unmagnetized fibers are unaffected by the magnetic control device, the total number of fibers not oriented towards the stress direction increases, thus further enhancing the tensile strength of the welded joint outside the preset stress direction.
[0263] The basic principles, main features, and advantages of this invention have been described above. Those skilled in the art should understand that this invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely principles of the invention. Various changes and modifications can be made without departing from the spirit and scope of the invention, and all such changes and modifications fall within the scope of the invention as claimed. The scope of protection claimed by this invention is defined by the appended claims and their equivalents.
Claims
1. A magnetic welding device, characterized in that, It includes: Equipment main frame (2), A welding operation platform (3) is installed on the main frame (2) of the equipment. The welding operation platform (3) includes a welding platform (31) and two clamps (32). The welding platform (31) is used to place the workpiece to be welded and to perform welding operations on the workpiece. The two clamps (32) are symmetrically installed on the welding platform (31) and are connected to each other by a heating element. A pressure output device (1) is installed on the main frame (2) of the equipment and faces the welding operation platform (3). The pressure output device (1) includes a cylinder (11) and a pressure head (12). The pressure head (12) is connected to the cylinder (11). The cylinder (11) can drive the pressure head (12) to move towards the workpiece to be welded placed on the welding platform (31) until it contacts the workpiece to be welded and applies pressure to the workpiece to be welded. A magnetic control device (4) is installed on the main frame (2) of the equipment. The magnetic control device (4) includes a ring electromagnet, a mounting bracket (41) for placing the ring electromagnet, and a steering mechanism. The mounting bracket (41) is connected to the steering mechanism. The steering mechanism is adapted to drive the ring electromagnet to turn through the mounting bracket (41) so that the direction of the magnetic field generated by the ring electromagnet is consistent with the direction of the force on the workpiece to be welded. The control device (5) includes a welding current control component (52), a welding pressure control component (51), and an electromagnetic field strength control component (53). The two ends of the welding current control component (52) are respectively connected to two clamps (32) so that the welding current control component (52), the two clamps (32), and the heating element form an electrical circuit. The welding pressure control component (51) is electrically connected to the pressure output device (1) and is used to control the output pressure of the welding pressure control component (51). The electromagnetic field strength control component (53) is electrically connected to the annular electromagnet and is used to control the magnetic field strength of the annular electromagnet. The steering mechanism includes a first support ring (42), a second support ring (43), two second mounting brackets (44), a first drive component (45), and a second drive component (46). The first support ring (42) is provided with multiple support columns (421), which are fixedly installed on the main frame (2) of the equipment. The outer diameter of the second support ring (43) is smaller than the inner diameter of the first support ring (42), and the second support ring (43) is slidably installed on the inner side of the first support ring (42). The first drive component (45) is connected to the first support ring (46). Ring 2 (43), the driving component 1 (45) can drive the support ring 2 (43) to rotate along the axial direction of the support ring 1 (42); two mounting brackets 2 (44) are symmetrically mounted on the support ring 2 (43), the two ends of the mounting bracket 1 (41) are respectively rotatably mounted on the two mounting brackets 2 (44), the driving component 2 (46) is connected to the mounting bracket 1 (41), the driving component 2 (46) can drive the mounting bracket 1 (41) to rotate along the radial direction of the support ring 1 (42).
2. The magnetic welding equipment as described in claim 1, characterized in that, The magnetic control welding equipment also includes a computer control terminal (6), which is connected to the control device (5) and the magnetic control device (4) respectively. The computer control terminal (6) is used to monitor and record the welding current of the welding current control component (52), the welding voltage of the welding pressure control component (51) and the magnetic field strength of the electromagnetic field strength control component (53) in real time, and to control the magnetic control device (4) to rotate by controlling the steering mechanism.
3. The magnetic welding equipment as described in claim 1, characterized in that, The distance from the welding platform (31) to the bottom of the main frame (2) of the equipment is equal to the distance from the annular electromagnet to the bottom of the main frame (2) of the equipment, and the center of the annular electromagnet coincides with the center point of the welding platform (31).
4. The magnetic welding equipment as described in claim 1, characterized in that, The welding operation platform (3) also includes a welding support frame (33) and a base (34). One end of the welding support frame (33) is connected to the welding platform (31), and the other end of the welding support frame (33) is connected to the base (34). The base (34) is fixedly installed on the main frame (2) of the equipment.
5. The magnetic welding equipment as described in claim 1, characterized in that, The welding current control component (52) includes a display screen (521), a display screen (522), an adjustment knob (524), and a switch (523). The display screen (521), the display screen (522), the adjustment knob (524), and the switch (523) are all installed on the control panel of the control device (5). The display screen (521) is suitable for displaying real-time data of the welding voltage during the welding process. The display screen (522) is suitable for displaying real-time data of the welding current during the welding process. The adjustment knob (524) is used to adjust the current value during the welding process. The switch (523) is suitable for controlling the opening or closing of the entire welding current control component (52).
6. The magnetic welding equipment as described in claim 1, characterized in that, The welding pressure control assembly (51) includes a display screen (514), a control knob (511), a pressure knob (512), an adjustment knob (513), and a switch. The display screen (514), the control knob (511), the pressure knob (512), the adjustment knob (513), and the switch are all installed on the control panel of the control device (5). The display screen (514) is adapted to display the preset pressure value of the pressure output device (1) during welding. The control knob (511) is adapted to control the cylinder (11) to drive the pressure head (12) to move up and down. The pressure knob (512) is adapted to adjust the pressure of the pressure output device (1) to the preset pressure value displayed on the display screen (514). The adjustment knob (513) is used to adjust the preset pressure value displayed on the display screen (514). The switch is adapted to control the opening or closing of the entire welding pressure control assembly (51).
7. The magnetic welding equipment as described in claim 1, characterized in that, The electromagnetic field strength control component (53) includes a fourth display screen (531), a fifth display screen (532), an adjustment knob (534), and a third switch (533). The fourth display screen (531), the fifth display screen (532), the adjustment knob (534), and the third switch (533) are all installed on the control panel of the control device (5). The fourth display screen (531) is adapted to display the real-time voltage of the magnetic field generated by the annular electromagnet. The fifth display screen (532) is adapted to display the real-time current of the magnetic field generated by the annular electromagnet. The adjustment knob (534) is used to adjust the current value displayed on the fifth display screen (532). The third switch (533) is adapted to control the opening or closing of the entire electromagnetic field strength control component (53).
8. The magnetic welding equipment as described in claim 1, characterized in that, The control device (5) is also equipped with a power supply, which is connected to the welding current control component (52), the welding pressure control component (51) and the electromagnetic field strength control component (53) respectively, so as to supply power to the welding current control component (52), the welding pressure control component (51) and the electromagnetic field strength control component (53) respectively.
9. A welding method using the magnetic welding equipment as described in any one of claims 1-8, characterized in that, It includes the following steps: S1, two workpieces to be welded are clamped in a single lap joint, with one workpiece placed above the heating element and the other workpiece placed below the heating element; S2, connect the two ends of the heating element to the two clamps of the magnetic welding equipment respectively, so that the heating element, the two clamps and the welding current control component form an electrical circuit; S3, the pressure head in the pressure output device is slowly lowered to press against the welding joint of the two parts to be welded by the welding pressure control component, and then the pressure of the pressure output device is adjusted to the preset pressure value; S4. Based on the force direction of the two workpieces to be welded at the welding joint, the magnetic field direction of the annular electromagnet is adjusted through the steering mechanism so that the magnetic field direction of the annular electromagnet is consistent with the force direction of the welding joint; then the current of the electromagnetic field strength control component is adjusted so that the magnetic field strength of the annular electromagnet reaches the preset value. S5, start the welding current control component, and then adjust the current value of the welding current control component to the preset value to start the welding operation; S6. After welding is completed, first turn off the welding current control component. At this time, the electromagnetic field strength control component and the welding pressure control component continue to work. After the pressure and magnetism are maintained for a period of time, first turn off the electromagnetic field strength control component and then turn off the welding pressure control component.
10. The welding method of the magnetic welding equipment as described in claim 9, characterized in that, During the welding process, the temperature of the heating element is calculated using the following formula: ; Among them, T He The heating element temperature is represented by I, the current magnitude by R, the resistance of the heating element by A, and the heat dissipation area by T. r The value represents room temperature, and η1 represents heat dissipation efficiency, η1 = 20~30 W / (m•K); The formula for calculating welding time during the welding process is: t H =2Q / KL 搭 ; Among them, t H Where is the welding time, Q is the specific heat capacity of the workpiece to be welded, K is the thermal conductivity of the workpiece to be welded, and L is the welding time. 搭 This refers to the overlap distance of the workpieces to be welded along the direction of the heating element. Welding pressure is inversely proportional to the porosity of the heating element and inversely proportional to the temperature of the workpiece. The empirical formula for calculating welding pressure is as follows: ; Where P is the welding pressure and ζ is an empirical coefficient. T represents the porosity of the heating element. He The temperature of the heating element; The formula for calculating the magnetic field strength of the ring electromagnet is: H = N × I / L; Where H is the magnetic field strength of the ring electromagnet, with units of A / m, N is the number of turns of the coil, I is the current flowing through the coil, and L is the length of the coil; The formula for the magnitude of the force on the workpiece in the magnetic field is: F 磁 =m*x*V*H; Where m is the mass of the workpiece to be welded, x is the specific magnetization coefficient of the magnetic fiber, and the calculation formula is k*ρ, where k is the volume magnetic susceptibility, ρ is the density, V is the volume of the magnetic fiber, and H is the magnetic field strength of the ring electromagnet. The formula for the magnitude of the torque experienced by the workpiece in the magnetic field is: M=F 磁 *0.25L 纤维 Where M is the magnitude of the torque experienced by the magnetic fiber in the magnetic field, and L 纤维 F represents the length of the fiber. 磁 This represents the magnitude of the force exerted on the magnetic fiber in the magnetic field.
11. The welding method of the magnetic welding equipment as described in claim 10, characterized in that, The formula for calculating the holding time after welding is as follows: ; Where t represents the holding time, I represents the current value in the welding pressure control component, R represents the resistance value of the heating element, and T He T represents the temperature of the heating element. r Let A represent the room temperature, A represent the heat dissipation area, and t represent the heat dissipation area. H The welding time is indicated by η1, which represents the heat dissipation efficiency of the heating element through the workpiece to the air, η1 = 20~30 W / (m·K); η2 represents the heat dissipation efficiency of the welded joint, η2 = 18~25 W / (m·K).
Citation Information
Patent Citations
Magnetic field induction welding method