Copper-liquid metal composite thermal interface material and preparation method thereof
Through the preparation of copper-liquid metal composite materials, the problems of dissolution of traditional thermal interface materials in coolant and leakage and corrosion of liquid metal are solved, achieving high thermal conductivity and stability, and extending service life.
Patent Information
- Application Number
- CN202410949104.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Traditional polymer thermal interface materials are easy to swell and dissolve in coolant, while liquid metal thermal interface materials are easy to flow, leak and corrode, affecting their performance and service life.
Using the preparation method of copper-liquid metal composite thermal interface material, through copper foil edge sealing, coating with liquid metal and stacking, combined with high temperature or high and low temperature cycle processing, a high thermal conductivity and stable copper-liquid metal composite material is formed to prevent liquid Metal leakage and corrosion.
It achieves high thermal conductivity that is not decomposed in the coolant, improves the filling and stability of the material, extends the service life, and solves the problems of dissolution, leakage and corrosion of traditional materials.
Smart Images

Figure CN118752886A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal interface materials, and in particular to a copper-liquid metal composite thermal interface material and a preparation method thereof. Background Art
[0002] As the demand for computing power continues to increase in recent years, the heat generated by chips is also increasing rapidly. The heat dissipation method of servers has gradually changed from air cooling to immersion liquid cooling. Traditional polymer thermal conductive interface materials are easy to swell and dissolve in the coolant. Studies have shown that 55% of the failures of electronic equipment are caused by temperature, and the reliability of electronic components will decrease by 10% for every 2°C increase in temperature, leading to problems such as breakdown, stress mismatch, and solder joint cracking. Therefore, with the increasing demand for immersion liquid cooling, a thermal conductive material that is compatible with all coolants is needed to adapt to the application environment of immersion liquid cooling.
[0003] Existing liquid metal thermal interface materials are prone to flow and leakage, resulting in poor filling of the material, which affects the performance of the liquid metal thermal interface material. At the same time, liquid metal thermal interface materials are also prone to corrosion, which causes corrosion and aging of devices and affects their service life.
[0004] At present, there is an urgent need to provide a new method for preparing liquid metal composite thermal interface materials to solve the problems that traditional polymer thermal conductive interface materials are easy to swell and dissolve in coolant; existing liquid metal thermal interface materials are easy to flow and leak, affecting the performance of liquid metal thermal interface materials; and liquid metal thermal interface materials are easy to corrode, causing corrosion and aging of devices, affecting service life, etc. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a copper-liquid metal composite thermal interface material and a preparation method thereof. The copper-liquid metal composite thermal interface material provided by the present invention is different from common thermal interface materials, does not undergo overall phase change, will not be washed away by coolant, liquid metal does not leak or corrode, and the thermal interface material has good filling properties and high thermal conductivity.
[0006] In order to achieve the above objectives, the technical solution of the present invention is as follows.
[0007] In the first aspect, the preparation method of the copper-liquid metal composite thermal interface material provided by the present invention comprises: sealing the edge of the copper foil, then coating the surface of the copper foil with liquid metal to obtain the copper foil coated with liquid metal; then stacking the copper foil coated with liquid metal layer by layer, and fixing to obtain copper-liquid metal; and subjecting the copper-liquid metal to high temperature treatment or high and low temperature cycle treatment to obtain the copper-liquid metal composite thermal interface material. The preparation process of the copper-liquid metal composite thermal interface material provided by the present invention effectively ensures the efficient thermal conductivity and structural stability of the material through copper foil edge sealing, coating liquid metal, stacking and specific treatment. By reacting liquid metal with copper under high temperature or high and low temperature cycle conditions, a high thermal conductivity copper-liquid metal composite thermal interface material is obtained as an effective heat dissipation component to solve the existing technical problems of thermal interface materials; after copper and liquid metal are compounded, the thermal conductivity and stability of the composite thermal interface material can be improved. Compared with traditional polymer thermal conductive interface materials, it has a high thermal conductivity coefficient and will not be decomposed in the coolant, which solves the problem that traditional polymer thermal conductive interface materials are easy to swell and dissolve in immersion liquid cooling, causing breakdown, stress mismatch, and solder joint cracking; liquid metal reacts with copper to form an alloy, which improves the filling property of the material and solves the problem that the liquid metal of the existing liquid metal thermal interface material is easy to leak and corrode.
[0008] Preferably, the edges of the copper foil are sealed with high temperature resistant double-sided tape.
[0009] Preferably, the copper foil coated with liquid metal is stacked layer by layer to obtain a sandwich stacking structure, and a layer of copper foil not coated with liquid metal is covered on the upper and lower surfaces of the sandwich stacking structure, and copper-liquid metal is obtained after fixing. The sandwich stacking structure is formed by stacking copper foil coated with liquid metal, and the upper and lower surfaces are covered with copper foil not coated with liquid metal. This structural design further enhances the overall strength and stability of the material, while improving its thermal conductivity, ensuring the integrity of the material during high temperature treatment.
[0010] Further preferably, the method for preparing the copper-liquid metal composite thermal interface material comprises the following steps.
[0011] 1) Preparation of liquid metal.
[0012] 2) The edges of the copper foil are sealed with a high temperature resistant double-sided tape, and then liquid metal is coated inside the sealed copper foil, and the copper foils coated with liquid metal are stacked layer by layer to obtain a sandwich stacking structure.
[0013] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and the layers are fixed with a clamp to obtain copper-liquid metal.
[0014] 4) subjecting the copper-liquid metal to high temperature treatment or high and low temperature cycle treatment to obtain a copper-liquid metal composite thermal interface material. The above preparation steps can improve the quality of the final product.
[0015] Preferably, the liquid metal includes the following components in percentage by mass: 50-100% gallium, 0-50% indium, and 0-50% tin. The present invention uses liquid metal with a specific component ratio to ensure the characteristics and performance of the liquid metal, optimize the thermal conductivity and physical properties of the liquid metal, and better meet application requirements, thereby improving the applicability and flexibility of the material.
[0016] More preferably, the liquid metal is selected from one or more of Ga, GaIn, GaSn, and GaInSn. In the present invention, the use of the preferred liquid metal can ensure high thermal conductivity and chemical stability.
[0017] Preferably, the copper foil has a thickness of 0.03-1 mm.
[0018] Preferably, the liquid metal (single layer) coating thickness is 0.005-0.3 mm.
[0019] The present invention ensures that the copper foil is not easily deformed during the coating of liquid metal and high-temperature treatment by controlling the preferred thickness of the copper foil to 0.03-1 mm, thereby improving the overall performance and service life of the composite material, and ensuring the strength and thermal conductivity of the material. Reasonable control of the coating thickness can prevent the liquid metal from excessively flowing during the superposition process, maintain the consistency of the material, and optimize the thermal conductivity and stability of the material. By optimizing the copper foil thickness and the liquid metal coating thickness, the structural balance and thermal conductivity efficiency of the material are ensured, the mechanical properties and thermal conductivity of the material are optimized, and various problems caused by excessively thick or thin coatings are prevented.
[0020] Further preferably, the number of superimposed layers of the copper foil coated with liquid metal is 3 to 25 layers, preferably 4 to 8 layers. The present invention limits the preferred number of superimposed layers to ensure the thickness and performance stability of the composite material. By reasonably controlling the number of layers, the efficient thermal conductivity of the material can be ensured, and its mechanical strength and durability can be improved, making it perform better in practical applications.
[0021] Preferably, the high temperature treatment is performed at a temperature of 100-500° C. and for a time of 72-1000 h.
[0022] Preferably, the low temperature of the high-low temperature cycle treatment is -40~-30°C, the high temperature is 60~250°C, and the time is 100~1200h.
[0023] More preferably, the high-low temperature cycle treatment comprises: constant temperature treatment at -40 to -30°C for 0.5 to 1 hour, and then constant temperature treatment at 60 to 250°C for 0.5 to 1 hour, and repeating the operation 100 to 600 times.
[0024] In the present invention, by adopting high temperature treatment and high and low temperature cycle treatment under specific conditions, the material performance can be significantly improved, the stress inside the material can be effectively eliminated, and its heat resistance and thermal conductivity efficiency can be enhanced. At the same time, the stability and durability of the material under extreme temperature changes are optimized under high and low temperature cycle treatment, ensuring that the material can withstand frequent temperature fluctuations in practical applications and maintain stable physical and chemical properties. These processing steps enable the material to not only have excellent thermal conductivity, but also maintain long-term stability and reliability under extreme environmental conditions, and is suitable for various high-tech fields.
[0025] The second invention provides a copper-liquid metal composite thermal interface material, which is obtained by the preparation method of the copper-liquid metal composite thermal interface material.
[0026] Preferably, the thermal conductivity of the copper-liquid metal composite thermal interface material is greater than 67W / (m·K), and the contact thermal resistance is less than 0.06K.cm 2 / W.
[0027] Further preferably, the thermal conductivity of the copper-liquid metal composite thermal interface material is 80-156.5 W / (m·K), and the contact thermal resistance is less than 0.045 K.cm 2 / W.
[0028] The beneficial effects of the present invention are at least as follows: the high thermal conductivity copper-liquid metal composite thermal interface material and the preparation method thereof provided by the present invention, through the reaction of liquid metal with copper under high temperature or high and low temperature cycle conditions, the high thermal conductivity copper-liquid metal composite thermal interface material is obtained as an effective heat dissipation component to solve the existing technical problems of thermal interface materials; after copper and liquid metal are composited, the thermal conductivity and stability of the composite thermal interface material can be improved. Compared with traditional polymer thermal conductive interface materials, it has a high thermal conductivity coefficient and will not be decomposed in the coolant, which solves the problem that traditional polymer thermal conductive interface materials are easy to swell and dissolve in immersion liquid cooling, and cause breakdown, stress mismatch, and solder joint cracking; liquid metal reacts with copper to form an alloy, which improves the filling property of the material and solves the problem that the liquid metal of the existing liquid metal thermal interface material is easy to leak and corrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a microstructure diagram of the high thermal conductivity copper-liquid metal composite thermal interface material in Example 2. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In the embodiment of the present invention, the thermal conductivity test adopts GB / T22588-2008 standard and 25±1℃ environmental test. In the embodiment of the present invention, the fixture is fixed by a stainless steel (or carbon steel) metal plate with a thickness of 2~5mm and an outer dimension not less than the size of the copper foil. In the embodiment of the present invention, the liquid metal is evenly coated inside the cavity surrounded by the double-sided tape, and the single layer thickness of the liquid metal coating is 0.05~0.2mm.
[0033] Example 1
[0034] This embodiment provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0035] 1) Prepare liquid metal, heat 76 parts of Ga, 15 parts of In, and 9 parts of Sn to 100° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and after melting, cool to room temperature for use.
[0036] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.1 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and 5 pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0037] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0038] 4) placing the copper-liquid metal in a high temperature environment of 250° C. for reaction for 720 hours to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0039] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 89W / (m·K), and its contact thermal resistance is 0.032 K.cm 2 / W.
[0040] Example 2
[0041] This embodiment provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0042] 1) Prepare liquid metal, heat 100 parts of Ga to 35° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and the melting is completed and set aside.
[0043] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.05 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and 8 pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0044] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0045] 4) placing the copper-liquid metal in a -40-125°C high and low temperature circulation box, maintaining a constant temperature of -40°C for 30 minutes, and rapidly switching (each switching time is 5 seconds) to a constant temperature of 125°C for 30 minutes, and repeating this cycle 500 times to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0046] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 96W / (m·K), and its contact thermal resistance is 0.026 K.cm 2 / W. The microstructure of the high thermal conductivity copper-liquid metal composite thermal interface material provided in this embodiment is as follows Figure 1 shown.
[0047] Example 3
[0048] This embodiment provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0049] 1) Prepare liquid metal, heat 80 parts of Ga and 20 parts of In to 100° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and cool to room temperature after melting for use.
[0050] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.2 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and four pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0051] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0052] 4) placing the copper-liquid metal in a high temperature environment of 300° C. for reaction for 680 hours to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0053] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 91W / (m·K) and its contact thermal resistance is 0.027 K.cm 2 / W.
[0054] Example 4
[0055] This embodiment provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0056] 1) Prepare liquid metal, heat 85 parts of Ga and 15 parts of Sn to 100° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and cool to room temperature after melting for use.
[0057] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.2 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and 5 pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0058] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0059] 4) placing the copper-liquid metal in a -40-125°C high and low temperature circulation box, maintaining a constant temperature of -40°C for 45 minutes, and rapidly switching (each switching time is 5 seconds) to a constant temperature of 125°C for 45 minutes, and repeating this cycle 400 times to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0060] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 88W / (m·K), and its contact thermal resistance is 0.028 K.cm 2 / W.
[0061] Example 5
[0062] This embodiment provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0063] 1) Prepare liquid metal, heat 65 parts of Ga, 25 parts of In, and 10 parts of Sn to 100° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and after melting, cool to room temperature for use.
[0064] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.05 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and 6 pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0065] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0066] 4) placing the copper-liquid metal in a -40-125°C high and low temperature circulation box, maintaining a constant temperature of -40°C for 60 minutes, and rapidly switching (each switching time is 5 seconds) to a constant temperature of 125°C for 60 minutes, and repeating this cycle 200 times to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0067] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 83W / (m·K), and its contact thermal resistance is 0.024 K.cm 2 / W.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing a high thermal conductivity copper-liquid metal composite thermal interface material, comprising the following steps.
[0070] 1) Prepare liquid metal, heat 65 parts of Ga, 25 parts of In, and 10 parts of Sn to 100° C. and melt to obtain the liquid metal alloy, the melting time is 30 to 60 minutes, and after melting, cool to room temperature for use.
[0071] 2) A double-sided tape with a temperature resistance of 300° C. is attached to the edge of a copper foil with a thickness of 0.05 mm and a length and width of 15 cm to seal the edge, and the liquid metal is evenly coated on the inside, and 6 pieces of copper foil coated with the liquid metal are stacked layer by layer to form a sandwich stacking structure.
[0072] 3) A layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stack structure, and a clamp is used to fix the structure to prepare copper-liquid metal.
[0073] 4) The copper-liquid metal is placed in a -40~125°C high and low temperature circulation box, kept at a constant temperature of -40°C for 30 minutes, and quickly switched (each switching time is 5 seconds) to a constant temperature of 125°C for 30 minutes, and this cycle is repeated 80 times to obtain a high thermal conductivity copper-liquid metal composite thermal interface material.
[0074] The thermal conductivity of the resulting high thermal conductivity copper-liquid metal composite thermal interface material is 95W / (m·K) and its contact thermal resistance is 0.12 K.cm 2 / W. The only difference between this comparative example and Example 5 is the cycle time. Although the thermal conductivity is also within the scope of the present invention, the contact thermal resistance is 5 times that of Example 5, which cannot meet the use requirements and cannot achieve the use effect of traditional thermal interface materials.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a copper-liquid metal composite thermal interface material, characterized in that: include: The edges of the copper foil are sealed, and then liquid metal is coated on the surface of the copper foil to obtain a copper foil coated with liquid metal; then the copper foil coated with liquid metal is stacked layer by layer and fixed to obtain copper-liquid metal; the copper-liquid metal is subjected to high-temperature treatment or high-low temperature cycle treatment to obtain a copper-liquid metal composite thermal interface material.
2. The method for preparing the copper-liquid metal composite thermal interface material according to claim 1, characterized in that: The edges of the copper foil are sealed with high temperature resistant double-sided tape.
3. The method for preparing the copper-liquid metal composite thermal interface material according to claim 1 or 2, characterized in that: The copper foils coated with liquid metal are stacked layer by layer to obtain a sandwich stacking structure, and a layer of copper foil not coated with liquid metal is respectively covered on the upper and lower surfaces of the sandwich stacking structure, and the copper-liquid metal is obtained after fixing.
4. The method for preparing the copper-liquid metal composite thermal interface material according to claim 3, characterized in that: The following steps are involved: 1) Preparation of liquid metal; 2) The edges of the copper foil are sealed with a high temperature resistant double-sided adhesive, and then liquid metal is coated inside the sealed copper foil, and the copper foils coated with liquid metal are stacked layer by layer to obtain a sandwich stacking structure; 3) Covering the upper and lower surfaces of the sandwich stack structure with a layer of copper foil not coated with liquid metal, and fixing them with a clamp to obtain copper-liquid metal; 4) subjecting the copper-liquid metal to high temperature treatment or high and low temperature cycle treatment to obtain a copper-liquid metal composite thermal interface material.
5. The method for preparing the copper-liquid metal composite thermal interface material according to any one of claims 1 to 4, characterized in that: The liquid metal comprises the following components in percentage by mass: 50-100% gallium, 0-50% indium, and 0-50% tin.
6. The method for preparing the copper-liquid metal composite thermal interface material according to claim 5, characterized in that: The liquid metal is selected from one or more of Ga, GaIn, GaSn, and GaInSn.
7. The method for preparing the copper-liquid metal composite thermal interface material according to any one of claims 1 to 6, characterized in that: The copper foil thickness is 0.03-1 mm; And / or, the single layer thickness of the liquid metal coating is 0.005-0.3 mm.
8. The method for preparing the copper-liquid metal composite thermal interface material according to any one of claims 1 to 7, characterized in that: The high temperature treatment is performed at a temperature of 100-500°C and a time of 72-1000 hours; And / or, the low temperature of the high and low temperature cycle treatment is -40~-30°C, the high temperature is 60~250°C, and the time is 100~1200h; Preferably, the high-low temperature cycle treatment comprises: constant temperature treatment at -40 to -30°C for 0.5 to 1 hour, and then constant temperature treatment at 60 to 250°C for 0.5 to 1 hour, and repeating the operation 100 to 600 times.
9. A copper-liquid metal composite thermal interface material, characterized in that: The preparation method of the copper-liquid metal composite thermal interface material according to any one of claims 1 to 8 is obtained.
10. The copper-liquid metal composite thermal interface material according to claim 9, characterized in that: The thermal conductivity of the copper-liquid metal composite thermal interface material is greater than 67W / (m·K), and the contact thermal resistance is less than 0.06K.cm 2 / W.
Citation Information
Patent Citations
Nano porous copper liquid metal composite thermal interface material and preparation method thereof
CN113201660A
Phase-change heat-conducting gasket as well as preparation process and application thereof
CN117558690A
Method for applying liquid metal as thermal interface material
CN117736700A
Multilayer heat conduction piece
CN209845582U
Liquid metal particle coating sheet member having electromagnetic wave shielding function and heat dissipation function and method of preparing the same
KR102047831B1