Biochar as well as preparation method and application thereof
Through the hydrothermal coupling acid strengthening method, low-concentration nitric acid and phosphorus-containing sodium salt react with straw under subcritical conditions, solving the problems of ash clogging and environmental pollution in traditional methods, and improving the active sites and energy storage performance of biochar. .
Patent Information
- Application Number
- CN202411251712.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the traditional straw carbonization process, ash blocks the pore structure, affecting the activation effect and conductive properties. Moreover, the pickling deashing method has environmental pollution problems and the number of active sites of biochar is insufficient.
Using a hydrothermal coupling acid strengthening method, low-concentration nitric acid solution and phosphorus-containing sodium salt react with straw in subcritical water to remove ash and dope nitrogen and phosphorus to increase the number of active sites and pore structure of biochar.
Effectively remove straw ash, increase the specific surface area and number of active sites of biochar, reduce environmental pollution, and improve conductive properties and energy storage performance.
Smart Images

Figure CN118754121A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy storage materials, and in particular to biochar and a preparation method and application thereof. Background Art
[0002] The development of high-performance, environmentally friendly, renewable carbon sources and the efficient preparation of energy storage carbon materials are the research focuses of new energy development. The synthesis of energy storage carbon materials based on biomass-derived carbon sources has attracted widespread attention due to its well-developed pore structure and easy directional control of the doping process.
[0003] As a fibrous biomass, the main components of straw include cellulose, hemicellulose and lignin, etc. It is rich in resources, cheap and easy to obtain, and renewable. At the same time, in order to ensure the absorption and transportation of components such as water, ions and nutrients during the growth of crops, straw has formed multi-component, multi-dimensional, high carbon content and fine morphological structure. Porous carbon electrode materials with high specific surface area and rich pore structure can be obtained through simple carbonization and activation. However, straw contains a lot of ash, which is prone to mineralization reaction during carbonization and activation, thereby blocking some pore structures of biochar and affecting the activation effect. At the same time, as an electrode material, it will also affect the conductive properties, hinder the transmission of charged ions, and increase the chemical internal resistance of supercapacitors.
[0004] In traditional deashing strategies, acid washing and alkaline washing are mostly used. The acid concentration used in acid washing is high, which can easily cause environmental pollution and is not conducive to sustainable development. In addition, the number of active sites of the obtained biochar needs to be improved. Summary of the invention
[0005] The present invention provides a biochar and a preparation method and application thereof. The acid used in the present invention has a low concentration and achieves modification of the biochar while removing the ash of the biochar, and the modification increases the number of active sites of the biochar.
[0006] The present invention provides a method for preparing biochar by hydrothermal coupling acid-enhanced straw deashing and modification, comprising the following steps: The straw, nitric acid solution and sodium salt containing P are mixed, and the obtained mixture is subjected to a hydrothermal carbonization reaction to obtain biochar; During the hydrothermal carbonization reaction, the water in the mixture is in a subcritical state; The concentration of the nitric acid solution is 0.005-0.01 mol / L.
[0007] Preferably, the particle size of the straw is 10-80 mesh.
[0008] Preferably, the straw comprises corn straw.
[0009] Preferably, the solid-liquid ratio of the straw to the nitric acid solution is 1:10-20.
[0010] Preferably, the P-containing sodium salt includes one or more of Na2HPO4, NaH2PO4 and Na3PO4.
[0011] Preferably, the weight ratio of the P-containing sodium salt to the straw is 1:2-4.
[0012] Preferably, the temperature of the hydrothermal carbonization reaction is 150-200° C., the pressure is 10-15 MPa, and the time is 60-120 min.
[0013] Preferably, after the hydrothermal carbonization reaction, the process further comprises: performing solid-liquid separation on the obtained reaction product, and then drying the obtained solid to obtain the biochar; and recycling the liquid obtained from the solid-liquid separation into the hydrothermal carbonization reaction.
[0014] The present invention also provides biochar prepared by the method described in the above technical solution, wherein the biochar is doped with N and P; the ash content of the biochar is 0.3-0.9wt%, and the specific surface area is 500-600m 2 / g.
[0015] The present invention also provides the application of the biochar described in the above technical solution in the field of energy storage.
[0016] The present invention provides a method for preparing biochar by hydrothermal coupling acid-enhanced straw deashing, comprising the following steps: The straw, nitric acid solution and sodium salt containing P are mixed and subjected to hydrothermal carbonization reaction to obtain N- and P-doped biochar; During the hydrothermal carbonization reaction, water in the mixture obtained by mixing is in a subcritical state; The concentration of the nitric acid solution is 0.005-0.01 mol / L.
[0017] In the present invention, the reaction system in which water is in a subcritical state strengthens the removal of soluble ash (alkaline earth metals such as K salts, Ca salts, and Mg salts) in straw by HNO3, and reduces the concentration of nitric acid solution; the sodium ions produced by the P-containing sodium salt are beneficial to the removal of ash of insoluble substances such as SiO2 in the straw, and at the same time have a certain activation effect on the biochar, further improving the pore structure; and when the water is in a subcritical state, N produced by HNO3 and P produced by the P-containing sodium salt are doped into the biochar. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a process flow chart of an embodiment; Figure 2 This is the SEM image of the biochar prepared in Example 1; Figure 3 The adsorption-desorption curve of the biochar prepared in Example 1; Figure 4 This is the pore size distribution diagram of the biochar prepared in Example 1. DETAILED DESCRIPTION
[0019] The present invention provides a method for preparing biochar by hydrothermal coupling acid-enhanced straw deashing, comprising the following steps: The straw, nitric acid solution and sodium salt containing P are mixed and subjected to hydrothermal carbonization reaction to obtain N- and P-doped biochar; During the hydrothermal carbonization reaction, water in the mixture obtained by mixing is in a subcritical state; The concentration of the nitric acid solution is 0.005-0.01 mol / L.
[0020] In the present invention, the particle size of the straw is preferably 10-80 meshes, more preferably 20-60 meshes, and further preferably 30-50 meshes; the straw preferably includes corn straw.
[0021] In the present invention, the straw preparation method preferably comprises the following steps: washing, drying and crushing the straw raw material in sequence.
[0022] The present invention has no particular limitation on the cleaning, and the surface dust can be removed by using a solution well known to those skilled in the art.
[0023] In the present invention, the solid-liquid ratio of the straw to the nitric acid solution is preferably 1:10-20, more preferably 1:12-15; the solid-liquid ratio refers to the mass ratio; the concentration of the nitric acid solution is 0.005-0.01 mol / L. A low concentration of 0.005-0.01 mol / L HNO3 (10-20 times lower than the heat transfer pickling concentration) is selected: on the one hand, HNO3 is enhanced to remove soluble ash (alkaline earth metals such as K salts, Ca salts, and Mg salts) in the straw under high-pressure subcritical conditions; on the other hand, the N element produced by HNO3 under high-pressure subcritical conditions can be doped into the hydrothermal carbon skeleton to form N-doped carbon, further improving the hydrothermal carbon skeleton structure and surface groups.
[0024] In the present invention, the weight ratio of the sodium salt containing P to the straw is preferably 1:2-4, more preferably 1:2.5-3; the sodium salt containing P preferably includes one or more of Na2HPO4, NaH2PO4 and Na3PO4. The sodium ions produced by the sodium salt containing P are beneficial to the ash removal of insoluble substances such as SiO2 in the straw, and have a certain activation effect on the straw hydrochar, further improving the pore structure; in addition, the P element of the sodium salt containing P can be doped into the hydrochar skeleton to form P-doped carbon, further improving the surface groups and active sites of the hydrochar.
[0025] In the present invention, the temperature of the hydrothermal carbonization reaction is preferably 150-200°C, more preferably 160-180°C; the pressure is preferably 10-15MPa, more preferably 12-13MPa; the time is preferably 60-120min, more preferably 80-100min. The present invention controls the temperature and pressure of the hydrothermal carbonization reaction so that water is in a subcritical state.
[0026] After the hydrothermal carbonization reaction, the present invention preferably further comprises: solid-liquid separation of the obtained reaction product, and then washing and drying the obtained solid to obtain the biochar; the liquid obtained by the solid-liquid separation is preferably reused in the hydrothermal carbonization reaction after mixing.
[0027] The present invention has no special limitation on the washing, and conventional technical means can be used for washing until neutrality.
[0028] The present invention also provides biochar prepared by the method described in the above technical solution, wherein the biochar is doped with N and P; the ash content of the biochar is 0.3-0.9wt%, and the specific surface area is 500-600m 2 / g.
[0029] The present invention also provides the application of the biochar described in the above technical solution in the field of energy storage.
[0030] In the present invention, the application preferably includes: activating the biochar to generate porous carbon.
[0031] The biochar provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0032] The flowchart of the embodiment of the present invention is as follows Figure 1 As shown: the crop straw is pretreated and uniformly mixed with a modifier and a low-concentration acid and then hydrothermally carbonized. The product obtained by the hydrothermal carbonization is then separated into solid and liquid to obtain solid low-ash hydrothermal carbon; the obtained liquid is recycled.
[0033] Example 1 (1) Using corn stalks as raw materials, soak the corn stalks in tap water for 2 h, wash off the dust on the surface, and then put them into an oven for drying. The oven temperature is set to 105 °C and the drying time is 2 h. The dried raw materials are then crushed into 40-80 meshes for use as raw materials.
[0034] (2) The raw material obtained in step (1) is mixed evenly with a low-concentration acid and a modifier, and then placed in a hydrothermal carbonization reactor for hydrothermal carbonization treatment. The solid-liquid ratio of the raw material mass to the low-concentration acid is 1:20, the low-concentration acid is 0.01 mol / L HNO3, the modifier is Na2HPO4, and the weight ratio of Na2HPO4 to straw is 1:2.
[0035] (3) Hydrothermal carbonization: A high-pressure and low-temperature hydrothermal carbonization treatment process was used, with a solid-liquid ratio of 1:20, a hydrothermal carbonization reaction temperature of 200°C, a hydrothermal carbonization reactor pressure of 10 MPa, and a reaction time of 120 min, so that the water in the hydrothermal reactor reached a subcritical reaction state, thereby promoting the penetration of acid ions.
[0036] (4) Water washing and drying treatment: The biochar obtained by hydrothermal conversion is washed with deionized water until it becomes neutral and then dried to obtain biochar.
[0037] In the hydrothermal conversion system, a low concentration of 0.01 mol / L HNO3 (10-20 times lower than the heat transfer acid washing concentration) is selected: on the one hand, HNO3 enhances the removal of soluble ash (alkaline earth metals such as K salts, Ca salts, and Mg salts) in straw under high-pressure subcritical conditions; on the other hand, the N element produced by HNO3 under high-pressure subcritical conditions can be doped into the hydrothermal carbon skeleton to form N-doped carbon, further improving the hydrothermal carbon skeleton structure and surface groups; Na2HPO4 is selected in the hydrothermal conversion system: on the one hand, the Na ions produced by Na2HPO4 are beneficial to the ash removal of insoluble substances such as SiO2 in the straw, and at the same time have a certain activation effect on the straw hydrothermal carbon, further improving the pore structure; on the other hand, the P element produced by Na2HPO4 can also be doped into the hydrothermal carbon skeleton to form P-doped carbon, further improving the surface groups and active sites of the hydrothermal carbon.
[0038] Under the combined action of low concentrations of HNO3 and Na2HPO4, and intensified in a high-pressure subcritical reaction system, the ash content of the straw hydrothermal charcoal can be reduced from the normal 10% to 0.5%, and the specific surface area of the biochar can reach 500-600m 2 / g, and the surface has N and P loaded functional groups.
[0039] The biochar prepared in Example 1 was subjected to SEM analysis, and the results were as follows: Figure 2 shown.
[0040] Depend on Figure 2 It can be seen that a rich microporous morphology structure is formed on the surface of biochar, and the pores are relatively uniform, indicating that the biochar has good activated carbon quality.
[0041] The adsorption-desorption curve of biochar is as follows Figure 3 As shown, the pore size distribution is Figure 4 shown.
[0042] Depend on Figure 3 It can be seen that biochar exhibits the curve structure of type I activated carbon and contains a relatively obvious hysteresis loop, indicating that it also has a certain mesoporous structure.
[0043] Depend on Figure 4 It can be seen that the biological pore size is concentrated at around 2nm, which has good charged ion adsorption capacity and therefore has good energy storage characteristics.
[0044] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing biochar by hydrothermal coupled acid-enhanced straw deashing and modification, characterized in that: The following steps are involved: The straw, nitric acid solution and sodium salt containing P are mixed, and the obtained mixture is subjected to a hydrothermal carbonization reaction to obtain biochar; During the hydrothermal carbonization reaction, the water in the mixture is in a subcritical state; The concentration of the nitric acid solution is 0.005-0.01 mol / L.
2. The method according to claim 1, characterized in that The particle size of the straw is 10-80 meshes.
3. The method according to claim 1 or 2, characterized in that: The straw includes corn straw.
4. The method according to claim 1 or 2, characterized in that: The solid-to-liquid ratio of the straw to the nitric acid solution is 1:10-20.
5. The method according to claim 1 or 2, characterized in that: The P-containing sodium salt includes one or more of Na2HPO4, NaH2PO4 and Na3PO4.
6. The method according to claim 1, characterized in that The weight ratio of the P-containing sodium salt to the straw is 1:2-4.
7. The method according to claim 1, characterized in that The temperature of the hydrothermal carbonization reaction is 150-200° C., the pressure is 10-15 MPa, and the time is 60-120 min.
8. The method according to claim 1, characterized in that After the hydrothermal carbonization reaction, the method further includes: performing solid-liquid separation on the obtained reaction product, and then washing and drying the obtained solid to obtain the biochar; and recycling the liquid obtained from the solid-liquid separation into the hydrothermal carbonization reaction.
9. The biochar prepared by the method according to any one of claims 1 to 8, characterized in that: The biochar is doped with N and P; the ash content of the biochar is 0.3-0.9 wt % and the specific surface area is 500-600 m 2 / g.
10. Application of the biochar according to claim 9 in the field of energy storage.
Citation Information
Patent Citations
Preparation method of carboxylation hydrothermal biomass charcoal for remedying uranium-containing wastewater
CN104492382A
System and method for preparing straw nitrogen-phosphorus-iron co-doped activated carbon electrode material
CN111540617A
Method for preparing hierarchical-pore phosphorus-doped carbon material from biomass
CN112010302A
Iron-silver co-doped biochar with high adsorption capacity and preparation method of iron-silver co-doped biochar
CN114588872A
Enhanced biochar
US20180118631A1