High-insulation glass powder for automobile spark plug and preparation method of high-insulation glass powder

By precisely controlling the composition and crystal structure of glass powder, combined with special processing, amorphous glass powder with high insulation and high mechanical strength is formed, which solves the problem of insufficient heat resistance and mechanical strength of traditional glass powder in high temperature and high pressure environments. Significantly improves the insulation performance and service life of the spark plug.

CN118754448APending Publication Date: 2024-10-11JIANGSU HONGPU ELECTRONIC MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411032106.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional glass powder has problems such as insufficient heat resistance, low mechanical strength, and aging in high-temperature and high-pressure environments, which affects the insulation performance and service life of spark plugs.

Method used

Using high-insulation glass powder composed of SiO2, B2O3, Al2O3, Na2O, K2O, TiO2, ZnO, CaO, MgO and other components, through precise control of composition and crystal structure, combined with ball milling, melting, rapid quenching, molding and sintering processes, Forming amorphous glass powder with high insulation and high mechanical strength.

Benefits of technology

It significantly improves the insulation performance, volume resistivity and breakdown voltage of the spark plug, extends its service life, remains stable under high temperature and high pressure conditions, and improves the reliability and overall performance of the spark plug.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970185690000071
    Figure BDA0004970185690000071
Patent Text Reader

Abstract

The invention relates to high-insulation glass powder for an automobile spark plug and a preparation method of the high-insulation glass powder. The glass powder mainly comprises B2O3, SiO2, Al2O3 and a plurality of additives, wherein the crystal structure of the B2O3 is a trigonal system. By accurately controlling the proportion of each component and the preparation process, the prepared glass powder has higher volume resistivity and breakdown voltage, and shows excellent dielectric properties and stable physicochemical properties. The preparation method disclosed by the invention is simple and easy for industrial production, and the prepared glass powder can be mixed with a ceramic matrix material to form a spark plug with high insulating property and high mechanical strength. Experimental results show that compared with traditional spark plug glass powder, the high-insulation glass powder is remarkably improved in the aspects of insulation performance, dielectric property and mechanical strength, and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass powder preparation, and more particularly to a high-insulation glass powder for automobile spark plugs and a preparation method thereof. Background Art

[0002] Automobile spark plugs are key components in the engine ignition system. Their main function is to ignite the mixed gas in the cylinder through electric sparks at the engine ignition time, thereby pushing the piston to operate and driving the vehicle forward. The performance of the spark plug directly affects the efficiency of the engine and the driving performance of the vehicle, so high-quality spark plugs are the basis for ensuring the normal operation of the engine.

[0003] The insulation performance of a spark plug is one of its key indicators. The quality of the insulation performance directly affects the ignition efficiency and service life of the spark plug. Currently, the spark plug insulation materials on the market mainly include ceramics and glass. Among them, glass powder has gradually become an important insulation material due to its excellent insulation performance and processability.

[0004] However, traditional glass powder has some problems, such as insufficient heat resistance, low mechanical strength, and easy aging under high temperature and high pressure environment. These problems seriously affect the service life and performance of spark plugs. In order to improve the insulation performance and service life of spark plugs, the development of a high insulation glass powder has become an important research direction. Summary of the invention

[0005] In order to further improve the insulation performance of existing automobile spark plugs, the present invention provides a high-insulation glass powder for automobile spark plugs and a preparation method thereof, and the specific scheme is as follows:

[0006] A high-insulation glass powder for automobile spark plugs, the glass powder comprising the following components in percentage by weight: SiO 2 :60-70wt%;B 2 O 3 :10-20wt%;Al 2 O 2 :5-10wt%;Na 2 O: 5-10wt%; K 2 O: 2-5wt%; TiO 2 : 0.5-2wt%; ZnO: 0.5-2wt%; CaO: 1-3wt%; MgO: 0.5-1wt%.

[0007] Furthermore, the SiO 2 The average particle size is 2 to 5 μm.

[0008] Furthermore, the B 2 O3 The crystal structure of boron is trigonal, with oxygen atoms arranged in a hexagonal stacking structure and boron atoms located in the octahedral gap between two oxygen atomic layers.

[0009] Furthermore, Al 2 O 3 The crystal structure is hexagonal.

[0010] Furthermore, Na 2 The density of O is 2.0~2.5g / cm 3 .

[0011] Furthermore, the crystal structure of MgO is cubic.

[0012] A method for preparing high-insulation glass powder for automobile spark plugs, the preparation method comprising the following steps:

[0013] S1: The glass powder is prepared according to its weight percentage, and the raw materials are fully mixed using a ball mill, and the mixing time is controlled within 4 to 6 hours;

[0014] S2: placing the mixed raw materials in a high temperature furnace for melting, the melting temperature is controlled at 1500-1600°C, and the melting time is 2-3h;

[0015] S3: After melting, rapid quenching is performed immediately, using water quenching or air quenching to ensure the formation of uniform amorphous glass;

[0016] S4: Grinding the molten glass block into powder through ball milling and screening process, and the particle size is controlled at 1-10 μm;

[0017] S5: glass powder is mixed with ceramic matrix material at a ratio of 10-15 wt %; mixing is performed using a stirrer for 2-3 hours to ensure that the powder is evenly dispersed in the ceramic matrix;

[0018] S6: placing the mixed material in a mold and applying a pressure of 50 to 100 MPa for molding;

[0019] S7: The formed green body is placed in a high temperature furnace for sintering at a sintering temperature of 1300-1400° C. for a sintering time of 2-3 hours.

[0020] Furthermore, the ball milling medium in S4 is zirconia beads, and the ball milling time is controlled at 8 to 12 hours.

[0021] Furthermore, during sintering in S7, an inert gas is introduced into the sintering furnace.

[0022] Beneficial effects:

[0023] The present invention provides a high-insulation glass powder for automobile spark plugs and a preparation method thereof, which has the following beneficial effects compared with the prior art:

[0024] (1) By precisely controlling the composition and crystal structure of the glass powder, the prepared glass powder has a higher volume resistivity and breakdown voltage, which significantly improves the insulation performance of the spark plug and reduces the risk of electrical loss and arc jumping. 2 O 3 The crystal structure of B is trigonal, with oxygen atoms arranged in a hexagonal stacking structure and boron atoms located in the octahedral gap between two oxygen atomic layers. 2 O 3 This makes the glass powder have higher structural stability under high temperature and high pressure environment. The hexagonal stacking structure of oxygen atoms and the octahedral interstitial position of boron atoms ensure the high insulation and dielectric constant stability of the material, thereby significantly improving the insulation performance and service life of the spark plug. 2 O 3 It has high hardness and high thermal stability, which helps to improve the overall mechanical strength and heat resistance of glass powder. Cubic MgO has excellent electrical insulation and high melting point, which enables glass powder to maintain its insulation performance and physical stability under high temperature conditions.

[0025] (2) The glass powder in the present invention exhibits good stability in dielectric constant, which helps the spark plug to work stably under high temperature and high pressure conditions, thereby improving the reliability and service life of the spark plug.

[0026] (3) By optimizing the raw material ratio and preparation process, the glass powder forms a uniform amorphous structure during high-temperature melting and rapid quenching, ensuring the stability of its physical and chemical properties, thereby improving the overall performance of the spark plug. DETAILED DESCRIPTION

[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0028] Embodiment 1:

[0029] A high-insulation glass powder for automobile spark plugs, the glass powder comprising the following components in percentage by weight:

[0030] SiO 2 :65wt%;B 2 O 3 :15wt%;Al 2 O 3 :7wt%;Na 2O: 7wt%; K 2 O: 3wt%; TiO 2 : 1.5wt%; ZnO: 1wt%; CaO: 2wt%; MgO: 0.5wt%.

[0031] The preparation steps are as follows:

[0032] (1) Ingredients and mixing:

[0033] Weigh each component according to the above weight percentage; use a ball mill to mix, and control the mixing time to be 5 hours.

[0034] (2) Melting:

[0035] The mixed raw materials are placed in a high temperature furnace for melting; the melting temperature is set at 1550° C. and the melting time is 2.5 hours.

[0036] (3) Quenching:

[0037] After melting, the glass is quickly quenched by water quenching to form a uniform amorphous glass.

[0038] (4) Ball milling and screening:

[0039] The quenched glass block was ball-milled using zirconium oxide beads as ball-milling media; the ball-milling time was 10 hours, and the glass block was ground into a powder with an average particle size of 3 μm.

[0040] (5) Powder mixing:

[0041] The glass powder was mixed with the ceramic matrix material at a ratio of 15 wt %; a stirrer was used for mixing for 2.5 hours to ensure that the powder was evenly dispersed in the ceramic matrix.

[0042] (6) Molding: Place the mixed material in a mold and apply a pressure of 80 MPa for molding.

[0043] (7) Sintering:

[0044] The formed green body is placed in a high-temperature furnace for sintering; the sintering temperature is set at 1350°C and the sintering time is 2.5 hours; during the sintering process, an inert gas is introduced into the furnace to prevent oxidation of the material.

[0045] Embodiment 2:

[0046] A high-insulation glass powder for automobile spark plugs, the glass powder comprising the following components in percentage by weight: SiO 2 :68wt%;B 2 O 3 :12wt%;Al 2 O 3 :6wt%;Na2 O: 6wt%; K 2 O: 4wt%; TiO 2 : 1wt%; ZnO: 0.8wt%; CaO: 2.2wt%; MgO: 0.6wt%.

[0047] The preparation steps are as follows:

[0048] (1) Ingredients and mixing:

[0049] Weigh each component according to the above weight percentage; use a ball mill to mix, and control the mixing time to be 4.5 hours.

[0050] (2) Melting:

[0051] The mixed raw materials are placed in a high temperature furnace for melting; the melting temperature is set at 1520° C. and the melting time is 2.7 hours.

[0052] (3) Quenching:

[0053] Immediately after melting, the glass is rapidly quenched by air quenching to form a uniform amorphous glass.

[0054] (4) Ball milling and screening:

[0055] The quenched glass block was ball-milled using zirconium oxide beads as ball-milling media; the ball-milling time was 9 hours, and the glass block was ground into a powder with an average particle size of 4 μm.

[0056] (5) Powder mixing:

[0057] The glass powder was mixed with the ceramic matrix material at a ratio of 12 wt %; a stirrer was used for mixing for 2 hours to ensure that the powder was evenly dispersed in the ceramic matrix.

[0058] (6) Molding: Place the mixed material in a mold and apply a pressure of 70 MPa for molding.

[0059] (7) Sintering:

[0060] The formed green body is placed in a high-temperature furnace for sintering; the sintering temperature is set at 1370°C and the sintering time is 2.8 hours; during the sintering process, an inert gas is introduced into the furnace to prevent oxidation of the material.

[0061] Embodiment 3:

[0062] A high-insulation glass powder for automobile spark plugs, the glass powder comprising the following components in percentage by weight: SiO 2 :63wt%;B 2 O 3 :18wt%;Al 2 O3 :8wt%;Na 2 O: 6wt%; K 2 O: 3wt%; TiO 2 : 1.2wt%; ZnO: 1.2wt%; CaO: 2.5wt%; MgO: 0.6wt%.

[0063] The preparation steps are as follows:

[0064] (1) Ingredients and mixing:

[0065] Weigh each component according to the above weight percentage; use a ball mill to mix, and control the mixing time to be 6 hours.

[0066] (2) Melting:

[0067] The mixed raw materials are placed in a high temperature furnace for melting; the melting temperature is set at 1580°C and the melting time is 3 hours.

[0068] (3) Quenching:

[0069] After melting, the glass is quickly quenched by water quenching to form a uniform amorphous glass.

[0070] (4) Ball milling and screening:

[0071] The quenched glass block was ball-milled using zirconium oxide beads as ball-milling media; the ball-milling time was 12 hours, and the glass block was ground into a powder with an average particle size of 2.5 μm.

[0072] (5) Powder mixing:

[0073] The glass powder was mixed with the ceramic matrix material at a ratio of 10 wt %; a stirrer was used for mixing for 3 hours to ensure that the powder was evenly dispersed in the ceramic matrix.

[0074] (6) Molding: Place the mixed material in a mold and apply a pressure of 90 MPa for molding.

[0075] (7) Sintering:

[0076] The formed green body is placed in a high-temperature furnace for sintering; the sintering temperature is set at 1390°C and the sintering time is 3 hours; during the sintering process, an inert gas is introduced into the furnace to prevent oxidation of the material.

[0077] Comparative Example:

[0078] Uses traditional spark plug glass powder.

[0079] The insulation properties of the spark plug glass powders obtained in Examples 1 to 3 and the comparative example were tested, and the test results are shown in the following table:

[0080]

[0081] The test results show that compared with traditional spark plug glass powder, the high-insulation glass powder prepared in Example 1, Example 2 and Example 3 has significantly improved volume resistivity, dielectric constant and breakdown voltage, showing excellent insulation performance.

[0082] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-insulation glass powder for automobile spark plugs, characterized in that: The glass powder comprises the following components in weight percentage: SiO2: 60-70wt%; B2O3: 10-20wt%; Al2O3: 5-10wt%; Na2O: 5-10wt%; K2O: 2-5wt%; TiO2: 0.5-2wt%; ZnO: 0.5-2wt%; CaO: 1-3wt%; MgO: 0.5-1wt%.

2. The high-insulation glass powder for automobile spark plugs according to claim 1, characterized in that: The average particle size of the SiO2 is 2 to 5 μm.

3. The high-insulation glass powder for automobile spark plugs according to claim 1, characterized in that: The crystal structure of B2O3 is a trigonal system, oxygen atoms are arranged in a hexagonal stacking structure, and boron atoms are located in the octahedral gap between two oxygen atom layers.

4. The high-insulation glass powder for automobile spark plugs according to claim 1, characterized in that: The crystal structure of Al2O2 is hexagonal.

5. The high-insulation glass powder for automobile spark plugs according to claim 1, characterized in that: The density of Na2O is 2.0~2.5g / cm 3 .

6. The high-insulation glass powder for automobile spark plugs according to claim 1, characterized in that: The crystal structure of MgO is cubic.

7. A method for preparing high-insulation glass powder for automobile spark plugs, characterized in that: The preparation method comprises the following steps: S1: The glass powder is prepared according to its weight percentage, and the raw materials are fully mixed using a ball mill, and the mixing time is controlled within 4 to 6 hours; S2: placing the mixed raw materials in a high temperature furnace for melting, the melting temperature is controlled at 1500-1600°C, and the melting time is 2-3h; S3: After melting, rapid quenching is performed immediately, using water quenching or air quenching to ensure the formation of uniform amorphous glass; S4: Grinding the molten glass block into powder through ball milling and screening process, and the particle size is controlled at 1-10 μm; S5: glass powder is mixed with ceramic matrix material at a ratio of 10-15 wt %; mixing is performed using a stirrer for 2-3 hours to ensure that the powder is evenly dispersed in the ceramic matrix; S6: placing the mixed material in a mold and applying a pressure of 50 to 100 MPa for molding; S7: The formed green body is placed in a high temperature furnace for sintering at a sintering temperature of 1300-1400° C. for a sintering time of 2-3 hours.

8. The high-insulation glass powder for automobile spark plugs according to claim 7, characterized in that: The ball milling medium in S4 is zirconia beads, and the ball milling time is controlled at 8 to 12 hours.

9. The high-insulation glass powder for automobile spark plugs according to claim 7, characterized in that: During sintering in S7, an inert gas is introduced into the sintering furnace.

Citation Information

Patent Citations

  • Ceramic with improved high temperature electrical properties for use as a spark plug insulator

    CN101616878A

  • Ceramic with improved high temperature electrical properties for use as a spark plug insulator

    CN101717243A

  • Low temperature sintered glass-ceramic composite insulating material and preparation method thereof

    CN104844002A

  • Glass powder used for sealing of automotive spark plug and production method of glass powder used for sealing of automotive spark plug

    CN110627362A

  • Sparking plug

    CN1393968A