Corrosion-resistant glass fiber and preparation method thereof
Through high-temperature melting treatment and surface impregnation treatment of oxides in a specific proportion, the problem of corrosion of traditional glass fiber in acid and alkali environments is solved, its acid and alkali resistance and mechanical properties are improved, the preparation process is simplified, and it is suitable for high temperature environments. Broad application prospects.
Patent Information
- Application Number
- CN202410801893.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional glass fibers are prone to corrosion in acidic and alkaline environments, resulting in reduced mechanical properties and service life. The existing corrosion-resistant glass fiber preparation process is complex and costly, and the resulting products have poor mechanical properties and high temperature resistance, making it difficult to promote on a large scale. .
Using a specific proportion of silica, alumina, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide for high-temperature melting treatment, the glass fiber body is obtained by drawing, and surface impregnated, using silane coupling A mixed solution of coupling agent and fluoride is used for surface treatment to improve acid and alkali resistance.
Significantly improves the stability and service life of glass fiber in acid and alkali environments, enhances its strength and toughness, simplifies the preparation process, reduces costs, is suitable for high temperature environments, has excellent insulation properties and aging resistance, and is suitable for Various composite materials fields.
Smart Images

Figure BDA0004903614360000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass fibers, and in particular to a corrosion-resistant glass fiber and a preparation method thereof. Background Art
[0002] As an important composite material reinforcement, glass fiber is widely used in the fields of construction, transportation, electronics, aviation, etc. However, traditional glass fiber is prone to corrosion in acidic and alkaline environments, resulting in a decrease in its mechanical properties and service life.
[0003] In order to solve this problem, some corrosion-resistant glass fibers have appeared on the market, but their preparation cost is high, the process is complicated, and it is difficult to promote and use them on a large scale. In addition, the corrosion-resistant glass fibers produced have problems such as poor mechanical properties and poor high temperature resistance, and their application range is small. Therefore, it is of great practical significance and application prospects to develop a glass fiber with excellent corrosion resistance, simple preparation process and low cost. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a corrosion-resistant glass fiber and a preparation method thereof, so as to solve the problems that the existing corrosion-resistant glass fiber preparation process is complicated, and the corrosion-resistant glass fiber obtained has poor mechanical properties and poor high temperature resistance.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0007] Silicon dioxide 55%-65%, aluminum oxide 12%-18%, magnesium oxide 5%-10%, zirconium oxide 3%-7%, calcium oxide 8%-12%, sodium oxide 0.5%-2%, potassium oxide 0.5%-2% and titanium dioxide 1%-3%.
[0008] The beneficial effects of the present invention are as follows: the present invention provides a formula for preparing glass fiber, which significantly improves the stability of the glass fiber in an acidic or alkaline environment by introducing components such as zirconium oxide and titanium dioxide, thereby extending the service life of the glass fiber in an acidic or alkaline environment for a long time and improving the strength and toughness of the glass fiber.
[0009] Further, the following raw materials are included in weight percentage:
[0010] Silicon dioxide 58%-62%, aluminum oxide 12%-17%, magnesium oxide 5%-7%, zirconium oxide 3%-6%, calcium oxide 10%-12%, sodium oxide 1%-1.5%, potassium oxide 1%-1.5% and titanium dioxide 1%-3%.
[0011] Further, the following raw materials are included in weight percentage:
[0012] Silicon dioxide 61%, aluminum oxide 13%, magnesium oxide 6%, zirconium oxide 4%, calcium oxide 12%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 2%.
[0013] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0014] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to high-temperature melting treatment to obtain a molten raw material;
[0015] (2) drawing the molten raw material obtained in step (1) to obtain a glass fiber blank;
[0016] (3) The glass fiber blank obtained in step (2) is subjected to surface impregnation treatment, and then dried and solidified to obtain a product.
[0017] The beneficial effects of the present invention are as follows: the present invention is prepared by drawing in a molten state, and glass fibers of different diameters can be prepared as needed. By subjecting the drawn glass fiber blank to surface impregnation treatment, the acid and alkali resistance of the glass fiber is further improved. The preparation method is simple, easy to industrialize, and has high production efficiency, which meets the needs of large-scale industrial production.
[0018] Furthermore, the temperature of the high temperature melting treatment in step (1) is 1600-1700°C.
[0019] Furthermore, in step (2), the diameter of the glass fiber blank is 10-20 microns.
[0020] Furthermore, in step (3), a mixed solution of silane coupling agent and fluoride is used for surface immersion treatment, the mass fraction of the mixed solution is 1-5%, the mass ratio of the silane coupling agent to the fluoride is 1-5:1-5, and the surface immersion treatment time is 30-60 minutes.
[0021] The beneficial effect of adopting the above further technical solution is that the present invention performs surface treatment by using a mixed solution of a silane coupling agent and a fluoride, which has a better corrosion resistance effect than a single coating treatment method.
[0022] Furthermore, in step (3), the drying and curing temperature is 120-150° C. and the time is 2-4 hours.
[0023] The application of the above-mentioned corrosion-resistant glass fiber in the preparation of corrosion-resistant composite materials.
[0024] The present invention has the following beneficial effects:
[0025] (1) The present invention provides a corrosion-resistant glass fiber and a preparation method thereof. The corrosion-resistant glass fiber obtained shows significant advantages in corrosion resistance, mechanical properties, heat resistance, processing performance, economic cost, environmental performance, application range and process simplicity. It has higher chemical stability in acidic and alkaline environments, is not easily corroded, and has a longer service life. It shows better stability in high-temperature environments, is suitable for high-temperature working environments, has excellent thermal shock resistance, can be used in environments with sudden temperature changes, and also has excellent insulation performance, aging resistance and mechanical strength, and is suitable for a variety of composite material fields.
[0026] (2) The preparation method of the present invention is simple, easy to industrialize and produce, has high production efficiency, and meets the needs of large-scale industrial production. DETAILED DESCRIPTION
[0027] The principles and features of the present invention are described below in conjunction with the examples, which are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0028] Embodiment 1:
[0029] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0030] Silicon dioxide 60%, aluminum oxide 15%, magnesium oxide 7%, zirconium oxide 5%, calcium oxide 10%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 1%.
[0031] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0032] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1650° C. to obtain a molten raw material;
[0033] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 15 μm;
[0034] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 45 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0035] Embodiment 2:
[0036] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0037] Silicon dioxide 62%, aluminum oxide 12%, magnesium oxide 6%, zirconium oxide 6%, calcium oxide 10%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 2%.
[0038] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0039] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high temperature melting treatment at 1700° C. to obtain a molten raw material;
[0040] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 18 μm;
[0041] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 30 minutes, and then dried and cured at 140° C. for 2 hours to obtain a glass fiber blank.
[0042] Embodiment 3:
[0043] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0044] Silicon dioxide 58%, aluminum oxide 14%, magnesium oxide 7%, zirconium oxide 5%, calcium oxide 11%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 3%.
[0045] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0046] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1650° C. to obtain a molten raw material;
[0047] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 12 μm;
[0048] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 50 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0049] Embodiment 4:
[0050] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0051] Silicon dioxide 61%, aluminum oxide 13%, magnesium oxide 6%, zirconium oxide 4%, calcium oxide 12%, sodium oxide 1%, potassium oxide 0.5%-2% and titanium dioxide 1%-3%.
[0052] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0053] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1680° C. to obtain a molten raw material;
[0054] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 10 μm;
[0055] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 60 minutes, and then dried and cured at 40° C. for 2 hours to obtain a glass fiber blank.
[0056] Embodiment 5:
[0057] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0058] Silicon dioxide 59%, aluminum oxide 17%, magnesium oxide 5%, zirconium oxide 3%, calcium oxide 11%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 3%.
[0059] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0060] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1670° C. to obtain a molten raw material;
[0061] (2) pulling the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 20 μm;
[0062] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 45 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0063] Comparative Example 1:
[0064] A glass fiber comprising the following raw materials in percentage by weight:
[0065] Silicon dioxide 58%, aluminum oxide 16% and calcium oxide 26%.
[0066] The method for preparing the glass fiber comprises the following steps:
[0067] (1) mixing silicon dioxide, aluminum oxide and calcium oxide and subjecting them to high temperature melting treatment at 1650° C. to obtain a molten raw material;
[0068] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 15 μm;
[0069] (3) The glass fiber blank obtained in step (2) is surface-immersed in a mixed solution of silane coupling agent KH-560 and sodium fluoride with a total mass fraction of 3% (the mass ratio of silane coupling agent KH-560 to sodium fluoride is 1:1) for 45 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0070] Comparative Example 2:
[0071] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0072] Silicon dioxide 60%, aluminum oxide 15%, magnesium oxide 7%, zirconium oxide 5%, calcium oxide 10%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 1%.
[0073] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0074] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1650° C. to obtain a molten raw material;
[0075] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 15 μm;
[0076] (3) The glass fiber blank obtained in step (2) was immersed in a 3% by mass silane coupling agent KH-560 solution for 45 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0077] Comparative Example 3:
[0078] A corrosion-resistant glass fiber comprising the following raw materials in percentage by weight:
[0079] Silicon dioxide 60%, aluminum oxide 15%, magnesium oxide 7%, zirconium oxide 5%, calcium oxide 10%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 1%.
[0080] The method for preparing the corrosion-resistant glass fiber comprises the following steps:
[0081] (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment at 1650° C. to obtain a molten raw material;
[0082] (2) drawing the molten raw material obtained in step (1) through a platinum funnel to obtain a glass fiber blank with a diameter of 15 μm;
[0083] (3) The glass fiber blank obtained in step (2) is subjected to surface immersion treatment in a 3% by mass sodium fluoride solution for 45 minutes, and then dried and cured at 130° C. for 3 hours to obtain a glass fiber blank.
[0084] Test example:
[0085] The glass fibers prepared in Examples 1-5 and Comparative Example 1 were characterized. The glass fiber samples were immersed in a 10% sulfuric acid solution and a 10% sodium hydroxide solution for 24 hours, respectively, and their mass preservation rates were tested to characterize their acid resistance and alkali resistance; their tensile properties were tested by a universal mechanical tester; the glass fiber was kept at a certain ambient temperature for 30 minutes to observe whether the glass fiber had obvious deformation, and the temperature value at which the deformation occurred was recorded as its high temperature resistance performance parameter.
[0086] The experimental results are shown in Table 1.
[0087] Table 1 Performance characteristics
[0088]
[0089]
[0090] According to the data in the above table, compared with Comparative Example 1, the glass fiber prepared in the embodiment of the present invention has significantly stronger tensile strength and service life, and at the same time significantly improves the acid resistance, alkali resistance and high temperature resistance of the glass fiber, and improves the performance and application range of the glass fiber. Compared with the glass fibers treated with a single solute impregnation solution in Comparative Examples 2 and 3, the glass fibers prepared in the embodiment of the present invention have higher mechanical strength, acid and alkali resistance and high temperature resistance. In summary, the glass fibers prepared in the embodiment of the present invention have excellent insulation properties, anti-aging properties, mechanical strength and heat resistance, significantly improve the economic benefits of glass fibers, and have broad market application prospects and important practical value.
[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A corrosion-resistant glass fiber, characterized in that: The following raw materials are included in weight percentage: Silicon dioxide 55%-65%, aluminum oxide 12%-18%, magnesium oxide 5%-10%, zirconium oxide 3%-7%, calcium oxide 8%-12%, sodium oxide 0.5%-2%, potassium oxide 0.5%-2% and titanium dioxide 1%-3%.
2. The corrosion-resistant glass fiber according to claim 1, characterized in that: The following raw materials are included in weight percentage: Silicon dioxide 58%-62%, aluminum oxide 12%-17%, magnesium oxide 5%-7%, zirconium oxide 3%-6%, calcium oxide 10%-12%, sodium oxide 1%-1.5%, potassium oxide 1%-1.5% and titanium dioxide 1%-3%.
3. The corrosion-resistant glass fiber according to claim 2, characterized in that: The following raw materials are included in weight percentage: Silicon dioxide 61%, aluminum oxide 13%, magnesium oxide 6%, zirconium oxide 4%, calcium oxide 12%, sodium oxide 1%, potassium oxide 1% and titanium dioxide 2%.
4. The method for preparing the corrosion-resistant glass fiber according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) mixing silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, sodium oxide, potassium oxide and titanium dioxide and subjecting the mixture to a high-temperature melting treatment to obtain a molten raw material; (2) drawing the molten raw material obtained in step (1) to obtain a glass fiber blank; (3) The glass fiber blank obtained in step (2) is subjected to surface impregnation treatment, and then dried and solidified to obtain the product.
5. The method for preparing corrosion-resistant glass fiber according to claim 4, characterized in that: The temperature of the high temperature melting treatment in step (1) is 1600-1700°C.
6. The method for preparing corrosion-resistant glass fiber according to claim 4, characterized in that: In the step (2), the diameter of the glass fiber blank is 10-20 microns.
7. The method for preparing corrosion-resistant glass fiber according to claim 4, characterized in that: In the step (3), a mixed solution of silane coupling agent and fluoride is used for surface immersion treatment, the mass fraction of the mixed solution is 1-5%, the mass ratio of the silane coupling agent to the fluoride is 1-5:1-5, and the surface immersion treatment time is 30-60 minutes.
8. The method for preparing corrosion-resistant glass fiber according to claim 4, characterized in that: The drying and curing temperature in step (3) is 120-150° C. and the drying and curing time is 2-4 hours.
9. Use of the corrosion-resistant glass fiber according to any one of claims 1 to 3 in the preparation of corrosion-resistant composite materials.