Thinning liquid for cover plate glass containing high rare earth elements, thinning method and glass

By using hydrofluoric acid, ethyl acetate, sulfuric acid and perchloric acid thinning liquids, the problem of thinning high rare earth element cover glass is solved, and the effective thinning and surface performance improvement of the glass are achieved, which satisfies the needs of display screens, mobile phones requirements for applications such as cover plates.

CN118754453AActive Publication Date: 2024-10-11CAIHONG GRP SHAOYANG SPECIAL GLASS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410984291.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing glass thinning fluids cannot effectively thin high rare earth element cover glass, resulting in white attachments on the glass surface and poor performance, which cannot meet the application needs of components such as displays and mobile phone covers.

Method used

Provide a thinning liquid for cover glass containing high rare earth elements, including hydrofluoric acid, ethyl acetate, sulfuric acid, ethanol and perchloric acid. Through the combined action of these components, the glass network is corroded and catalyzed, and white attachments are inhibited. The generation ensures the transmittance and surface quality of the glass.

Benefits of technology

It achieves effective thinning of high rare earth element cover glass, avoids white attachments and flow mark defects, ensures the smoothness and transmittance of the glass surface, and meets the application needs of display screens, mobile phone covers and other components. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754453A_ABST
    Figure CN118754453A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high rare earth element cover plate glass thinning, in particular to a high rare earth element-containing cover plate glass thinning liquid, a high rare earth element-containing cover plate glass thinning method and high rare earth element-containing cover plate glass. The high rare earth element-containing cover plate glass thinning liquid comprises the following components in parts by mass: 10-20 parts of hydrofluoric acid, 10-20 parts of ethyl acetate, 10-15 parts of sulfuric acid, 5-10 parts of ethanol, 10-15 parts of perchloric acid and 25-65 parts of water. The glass network is eroded under the combined action of hydrofluoric acid and ethyl acetate, so that the glass network is disintegrated and thinned; by adding perchloric acid into the thinning liquid, the generation of hydrogen fluoride and yttrium oxide or yttrium hydroxide can be effectively inhibited, or the generated hydrogen fluoride and yttrium oxide or yttrium hydroxide are partially dissolved to inhibit or greatly reduce the generation of white attachments, thereby ensuring the transmittance of the thinned glass. Sulfuric acid can play a catalytic role, and the overall thinning speed is increased; and finally, under the combined action of ethyl acetate and ethanol, a good glass surface is obtained, so that the problems of flow mark-shaped defects, large surface roughness of the glass and the like are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thinning of cover glass containing high rare earth elements, and in particular to a thinning liquid for cover glass containing high rare earth elements, a thinning method and glass. Background Art

[0002] In order to enhance the hardness and toughness of the cover glass, high content of rare earth oxides such as yttrium oxide and lanthanum oxide are added to the new cover glass material.

[0003] The technical barriers of the one-shot molding method for high rare earth element cover glass are relatively high, and no manufacturer in the industry is currently able to achieve mass production. Due to the high barriers of the one-shot molding method, the mass production of high rare earth element cover glass can be achieved through the secondary molding process. The secondary molding process mainly uses chemical thinning and other methods to reduce the original glass sheet, thereby processing high-strength, high-modulus cover glass that meets the requirements.

[0004] Compared with common glass such as ordinary cover glass, the thinning of high rare earth element cover glass is more difficult. The thinning liquid disclosed in many documents is only suitable for ordinary glass. When one of them is directly used in the thinning process of high rare earth element cover glass, a large amount of white attachments appear on the glass surface. The composition is measured by EDS, and the main content weight percentage is: 50% F, 33% Y, and 4.2% Al. This is mainly due to the reaction of ordinary thinning liquid with high rare earth element cover glass. Hydrogen fluoride and yttrium oxide or yttrium hydroxide react to obtain yttrium fluoride, Y(OH)3+3HF→YF3+3H2O. There are also thinning liquids that react with high rare earth element cover glass to generate insoluble composite salts containing NH4F and YF3, which cannot meet the thinning requirements of high rare earth element cover glass. It cannot be used on display screens, mobile phone covers and other components. Summary of the invention

[0005] Aiming at the problem that the glass thinning liquid in the prior art cannot meet the thinning requirements of high rare earth element cover glass, the present invention provides a thinning liquid for cover glass containing high rare earth elements and a thinning method.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention provides a thinning liquid for cover glass containing high rare earth elements, which comprises, by mass, 10 to 20 parts of hydrofluoric acid, 10 to 20 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 5 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 65 parts of water.

[0008] Preferably, the mixture comprises, by mass: 15 to 20 parts of hydrofluoric acid, 10 to 15 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 8 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 55 parts of water.

[0009] Preferably, the mixture comprises, by mass: 20 parts of hydrofluoric acid, 13 parts of ethyl acetate, 14 parts of sulfuric acid, 10 parts of ethanol, 12 parts of perchloric acid and 31 parts of water.

[0010] The present invention also provides a method for thinning a cover glass containing a high amount of rare earth elements by using the above-mentioned thinning liquid, comprising:

[0011] Prepare the thinning liquid according to the mass components;

[0012] Pre-treating the cover glass containing high rare earth elements to be thinned to obtain an original cover glass containing high rare earth elements to be thinned;

[0013] The original sheet of cover glass containing high rare earth elements to be thinned is cleaned and dried to obtain a pre-treated cover glass containing high rare earth elements to be thinned;

[0014] The pre-treated cover glass containing high rare earth elements to be thinned is immersed in a thinning liquid for chemical thinning until the pre-treated cover glass containing high rare earth elements to be thinned reaches the target thickness, and the thinning is completed.

[0015] Preferably, the high rare earth element-containing cover glass to be thinned comprises, by mass, 30% to 42% SiO2, 20% to 40% Y2O3, 8% to 16% Al2O3 and 1% to 4% B2O3.

[0016] Preferably, the method of pre-treating the cover glass containing high rare earth elements to be thinned to obtain the original cover glass containing high rare earth elements to be thinned is:

[0017] The cover glass containing high rare earth elements to be thinned is sequentially precision-processed, ground and polished to obtain the original cover glass containing high rare earth elements to be thinned.

[0018] Preferably, the method for cleaning and drying the original sheet of cover glass containing high rare earth elements to be thinned to obtain the pre-treated cover glass containing high rare earth elements to be thinned is:

[0019] The original sheet of cover glass containing high rare earth elements to be thinned is washed with water, dried, then washed with mixed acid solution, dried, washed with water again, and dried to obtain the pre-treated cover glass containing high rare earth elements to be thinned.

[0020] Preferably, the mixed acid solution comprises, by mass, 10 to 15 parts of acetic acid, 10 to 15 parts of anhydrous ethanol and 70 to 80 parts of water.

[0021] Preferably, the temperature for chemical thinning is 45°C to 65°C.

[0022] A cover glass containing high rare earth elements is thinned by the above-mentioned thinning method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention provides a thinning liquid for cover glass containing high rare earth elements, which comprises, by mass, 10 to 20 parts of hydrofluoric acid, 10 to 20 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 5 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 65 parts of water. The glass network is corroded by the joint action of hydrofluoric acid and ethyl acetate, so that the glass network is disintegrated and thinned; by adding perchloric acid to the thinning liquid, the generation of hydrogen fluoride and yttrium oxide or yttrium hydroxide can be effectively inhibited, or the generated hydrogen fluoride and yttrium oxide or yttrium hydroxide can be partially dissolved to inhibit or greatly reduce the generation of white attachments, thereby ensuring the transmittance of the thinned glass. Sulfuric acid can play a catalytic role and increase the overall thinning speed; finally, under the joint action of ethyl acetate and ethanol, a good glass surface is obtained, thereby avoiding problems such as flow mark defects and large glass surface roughness, so as to meet the thinning requirements of cover glass containing high rare earth elements.

[0025] The thinning liquid for cover glass containing high rare earth elements comprises, by mass, 20 parts of hydrofluoric acid, 13 parts of ethyl acetate, 14 parts of sulfuric acid, 10 parts of ethanol, 12 parts of perchloric acid and 31 parts of water. The thinning liquid of this component can ensure the performance of the glass surface when the glass is thinned.

[0026] The present invention also provides a method for thinning a cover glass containing high rare earth elements by using the above-mentioned thinning liquid, wherein the method comprises preparing a thinning liquid, pre-treating, cleaning, and drying the cover glass containing high rare earth elements to be thinned, thereby obtaining a pre-treated cover glass containing high rare earth elements to be thinned; immersing the pre-treated cover glass containing high rare earth elements to be thinned in the thinning liquid, and performing chemical thinning until the pre-treated cover glass containing high rare earth elements to be thinned reaches the target thickness, thereby completing the thinning. The method is simple and easy to operate, suitable for industrial thinning, and the surface performance of the glass after thinning is good, which can meet the thinning requirements of the cover glass containing high rare earth elements.

[0027] The present invention also provides a cover glass containing high rare earth elements, which is thinned by the above-mentioned thinning method. After thinning, the surface of the glass has no white attachments, flow mark-like defects, high glass surface roughness and other problems, and meets the application requirements in display screens, mobile phone cover plates and other components. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a schematic flow chart of a method for thinning a cover glass containing high rare earth elements.

[0029] Figure 2 This is a real picture of the cover glass containing high rare earth elements after thinning according to Example 1 of the present invention.

[0030] Figure 3This is a real picture of the cover glass containing high rare earth elements after thinning in comparative example 1.

[0031] Figure 4 It is a comparison chart of the transmittance of the cover glass containing high rare earth elements after thinning in the embodiment of the present invention and the comparative example. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0033] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0034] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0038] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0039] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0040] The invention discloses a thinning liquid for cover glass containing high rare earth elements, which comprises, by mass, 10 to 20 parts of hydrofluoric acid, 10 to 20 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 5 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 65 parts of water.

[0041] Preferably, the thinning liquid for cover glass containing high rare earth elements comprises, by mass: 15-20 parts of hydrofluoric acid, 10-15 parts of ethyl acetate, 10-15 parts of sulfuric acid, 8-10 parts of ethanol, 10-15 parts of perchloric acid and 25-55 parts of water. Further preferably, it comprises, by mass: 20 parts of hydrofluoric acid, 13 parts of ethyl acetate, 14 parts of sulfuric acid, 10 parts of ethanol, 12 parts of perchloric acid and 31 parts of water.

[0042] See also Figure 1 The present invention provides a method for thinning a cover glass containing a high rare earth element by using the above-mentioned thinning liquid, comprising:

[0043] S1: Prepare the thinning liquid according to the mass components, specifically:

[0044] 10 to 20 parts of hydrofluoric acid, 10 to 20 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 5 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 65 parts of water are mixed uniformly to obtain a thinning solution;

[0045] S2: Pre-treating the cover glass containing high rare earth elements to be thinned to obtain the original cover glass containing high rare earth elements to be thinned, wherein the cover glass containing high rare earth elements to be thinned comprises, by mass, 30% to 42% SiO2, 20% to 40% Y2O3, 8% to 16% Al2O3 and 1% to 4% B2O3.

[0046] Specifically:

[0047] The cover glass containing high rare earth elements to be thinned is sequentially precision-processed, ground and polished to obtain an original cover glass containing high rare earth elements to be thinned;

[0048] S3: Cleaning and drying the original cover glass containing high rare earth elements to be thinned to obtain a pre-treated cover glass containing high rare earth elements to be thinned, specifically:

[0049] The original sheet of cover glass containing high rare earth elements to be thinned is washed with water, dried, then washed with mixed acid solution, dried, washed with water again, and dried to obtain the pre-treated cover glass containing high rare earth elements to be thinned; the mixed acid solution comprises, by mass, 10 to 15 parts of acetic acid, 10 to 15 parts of anhydrous ethanol and 70 to 80 parts of water; the mixed acid solution can effectively remove the substances attached to the surface of the cover glass containing high rare earth elements produced by grinding and polishing, and promote uniform reaction on the surface of the glass while cleaning the surface.

[0050] S4: Immerse the pretreated cover glass containing high rare earth elements to be thinned in a thinning liquid for chemical thinning until the pretreated cover glass containing high rare earth elements to be thinned reaches a target thickness and the thinning is completed. Specifically, immerse the pretreated cover glass containing high rare earth elements to be thinned in a thinning liquid for thinning at 45°C to 65°C for 1.5 to 2.5 hours.

[0051] Example 1

[0052] According to weight parts, 20 parts of hydrofluoric acid, 13 parts of ethyl acetate, 14 parts of sulfuric acid, 10 parts of ethanol, 12 parts of perchloric acid and 31 parts of water were mixed uniformly.

[0053] The original cover glass sheet containing high rare earth elements is processed by CNC (Computerized Numerical Control), ground and polished to form a 6-inch original cover glass sheet containing high rare earth elements with a thickness of 400um.

[0054] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0055] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 45°C and a chemical thinning time of 2.5 h.

[0056] After the thinned high rare earth element cover glass is cleaned and dried, a 30 μm high rare earth element cover glass is obtained. Figure 2 It can be seen that the surface of the high rare earth element cover glass has no white attachments and is smooth and delicate.

[0057] Example 2

[0058] According to weight parts, 15 parts of hydrofluoric acid, 15 parts of ethyl acetate, 15 parts of sulfuric acid, 10 parts of ethanol, 10 parts of perchloric acid and 35 parts of water were mixed uniformly.

[0059] The high rare earth element cover glass original sheet is processed by CNC, ground and polished to be a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0060] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0061] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 50°C and a chemical thinning time of 2.5 h.

[0062] The thinned high rare earth element cover glass is cleaned and dried to obtain a 30 μm high rare earth element cover glass. The actual surface of the high rare earth element cover glass obtained in this embodiment has no white attachments and is smooth and delicate.

[0063] Example 3

[0064] According to weight parts, 15 parts of hydrofluoric acid, 10 parts of ethyl acetate, 12 parts of sulfuric acid, 9 parts of ethanol, 3 parts of perchloric acid and 51 parts of water were mixed uniformly.

[0065] The high rare earth element cover glass original sheet is processed by CNC, ground and polished to be a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0066] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 12 parts of acetic acid, 13 parts of anhydrous ethanol, and 75 parts of water;

[0067] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 50°C and a chemical thinning time of 2.5 h.

[0068] The thinned high rare earth element cover glass is cleaned and dried to obtain a 30 μm high rare earth element cover glass. The actual surface of the high rare earth element cover glass obtained in this embodiment has no white attachments and is smooth and delicate.

[0069] Example 4

[0070] According to weight parts, 16 parts of hydrofluoric acid, 14 parts of ethyl acetate, 10 parts of sulfuric acid, 7 parts of ethanol, 13 parts of perchloric acid and 40 parts of water were mixed uniformly.

[0071] The high rare earth element cover glass original sheet is processed by CNC, ground and polished to be a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0072] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0073] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 46°C and a chemical thinning time of 2 hours;

[0074] The thinned high rare earth element cover glass is cleaned and dried to obtain a 30 μm high rare earth element cover glass. The actual surface of the high rare earth element cover glass obtained in this embodiment has no white attachments and is smooth and delicate.

[0075] Comparative Example 1

[0076] 10 parts of hydrofluoric acid, 10 parts of ammonium fluoride, 9 parts of citric acid, 13 parts of oxalic acid and 58 parts of water were mixed uniformly by mass to obtain a thinning solution.

[0077] The high rare earth element cover glass original sheet is processed by CNC, grinding and polishing to make a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0078] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0079] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 50°C and a chemical thinning time of 2.5 h.

[0080] After the thinned high rare earth element cover glass is cleaned and dried, a 30μm high rare earth element cover glass is obtained. Figure 3It can be seen from the actual picture of the soft high rare earth element cover glass obtained in this comparative example that white attachments are generated on the surface of the high rare earth element cover glass, and it cannot be used for display screens and mobile phone covers.

[0081] Comparative Example 2

[0082] 12 parts of hydrofluoric acid, 8 parts of ammonium fluoride, 9 parts of citric acid, 13 parts of oxalic acid and 58 parts of water were mixed uniformly by mass to obtain a thinning solution.

[0083] The high rare earth element cover glass original sheet is processed by CNC, grinding and polishing to make a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0084] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0085] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 50°C and a chemical thinning time of 2.5 h.

[0086] The thinned high rare earth element cover glass is cleaned and dried to obtain a 30 μm high rare earth element cover glass. The soft high rare earth element cover glass obtained in this comparative example has white attachments on its surface and cannot be used for display screens and mobile phone covers.

[0087] Comparative Example 3

[0088] 16 parts of hydrofluoric acid, 4 parts of ammonium fluoride, 9 parts of citric acid, 13 parts of oxalic acid and 58 parts of water were mixed uniformly by mass to obtain a thinning solution.

[0089] The high rare earth element cover glass original sheet is processed by CNC, grinding and polishing to make a 6-inch high rare earth element cover glass original sheet with a thickness of 400um.

[0090] The ground and polished high rare earth element cover glass original sheet is first washed with purified water and dried, then washed with a mixed acid solution for 5 minutes, and finally washed with purified water and dried to obtain a pre-treated high rare earth element cover glass to be thinned; wherein the mixed acid solution comprises, by weight: 10 parts of acetic acid, 10 parts of anhydrous ethanol, and 80 parts of water;

[0091] The 400 μm thick pre-treated cover glass containing high rare earth elements to be thinned was immersed in a thinning liquid with a temperature of 50°C and a chemical thinning time of 2.5 h.

[0092] The thinned high rare earth element cover glass is cleaned and dried to obtain a 30 μm high rare earth element cover glass. The soft high rare earth element cover glass obtained in this comparative example has white attachments on its surface and cannot be used for display screens and mobile phone covers.

[0093] The transmittance of the high rare earth element cover glass obtained in the above examples and comparative examples was tested, and the detection method and test results are as follows:

[0094] The glass transmittance was tested using a German Jena SPECORD50f spectrophotometer at a wavelength of 550nm:

[0095] High rare earth element cover glass Transmittance (%) High rare earth element cover glass original 88.80 Example 1 87.06 Example 2 86.72 Example 3 86.6 Example 4 86.7 Comparative Example 1 52.58 Comparative Example 2 55.99 Comparative Example 3 59.93

[0096] See also Figure 4 By comparing the transmittance of the cover glass containing high rare earth elements prepared in the embodiment and the comparative example, it can be seen that the transmittance of the glass thinned by the thinning liquid prepared by the present invention is almost unchanged compared with the original glass, which shows that the glass thinned by the thinning liquid of the present invention ensures the surface properties of the glass. However, the transmittance of the cover glass containing high rare earth elements after thinning by the comparative example, i.e. the existing thinning liquid, is seriously reduced, which seriously affects the subsequent application of the glass.

[0097] The present invention also provides a cover glass containing high rare earth elements, which is thinned by the above-mentioned thinning method. After thinning, the surface of the glass has no white attachments, flow mark-like defects, high glass surface roughness and other problems, and meets the application requirements in display screens, mobile phone cover plates and other components.

[0098] In summary, the present invention provides a thinning liquid, a thinning method and a glass for a cover glass containing high rare earth elements. The glass network is corroded by the joint action of hydrofluoric acid and ethyl acetate, so that the glass network is disintegrated and thinned; by adding perchloric acid to the thinning liquid, the generation of hydrogen fluoride and yttrium oxide or yttrium hydroxide can be effectively inhibited, or the generated hydrogen fluoride and yttrium oxide or yttrium hydroxide can be partially dissolved to inhibit or greatly reduce the generation of white attachments, thereby ensuring the transmittance of the thinned glass. Sulfuric acid can play a catalytic role and increase the overall thinning speed; finally, under the joint action of ethyl acetate and ethanol, a good glass surface is obtained, thereby avoiding problems such as flow mark defects and large glass surface roughness, so as to meet the thinning requirements of the cover glass containing high rare earth elements.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.

Claims

1. A thinning liquid for cover glass containing high rare earth elements, characterized in that: The composition comprises, by mass, 10 to 20 parts of hydrofluoric acid, 10 to 20 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 5 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 65 parts of water.

2. The thinning liquid for cover glass containing high rare earth elements according to claim 1, characterized in that: The composition comprises, by mass, 15 to 20 parts of hydrofluoric acid, 10 to 15 parts of ethyl acetate, 10 to 15 parts of sulfuric acid, 8 to 10 parts of ethanol, 10 to 15 parts of perchloric acid and 25 to 55 parts of water.

3. The thinning liquid for cover glass containing high rare earth elements according to claim 1 or 2, characterized in that: The components, by mass, include: 20 parts of hydrofluoric acid, 13 parts of ethyl acetate, 14 parts of sulfuric acid, 10 parts of ethanol, 12 parts of perchloric acid and 31 parts of water.

4. A method for thinning a cover glass containing high rare earth elements using the thinning liquid according to any one of claims 1 to 3, characterized in that: include: Prepare the thinning liquid according to the mass components; Pre-treating the cover glass containing high rare earth elements to be thinned to obtain an original cover glass containing high rare earth elements to be thinned; The original sheet of cover glass containing high rare earth elements to be thinned is cleaned and dried to obtain a pre-treated cover glass containing high rare earth elements to be thinned; The pre-treated cover glass containing high rare earth elements to be thinned is immersed in a thinning liquid for chemical thinning until the pre-treated cover glass containing high rare earth elements to be thinned reaches the target thickness, and the thinning is completed.

5. The method for thinning cover glass containing high rare earth elements according to claim 4, characterized in that: The high rare earth element-containing cover glass to be thinned comprises, by mass, 30% to 42% SiO2, 20% to 40% Y2O3, 8% to 16% Al2O3 and 1% to 4% B2O3.

6. The method for thinning cover glass containing high rare earth elements according to claim 4, characterized in that: The method of pre-treating the cover glass containing high rare earth elements to be thinned to obtain the original cover glass containing high rare earth elements to be thinned is as follows: The cover glass containing high rare earth elements to be thinned is sequentially precision-processed, ground and polished to obtain the original cover glass containing high rare earth elements to be thinned.

7. The method for thinning cover glass containing high rare earth elements according to claim 4, characterized in that: The method for cleaning and drying the original cover glass sheet containing high rare earth elements to be thinned to obtain the pre-treated cover glass containing high rare earth elements to be thinned is as follows: The original sheet of cover glass containing high rare earth elements to be thinned is washed with water, dried, then washed with mixed acid solution, dried, washed with water again, and dried to obtain the pre-treated cover glass containing high rare earth elements to be thinned.

8. The method for thinning cover glass containing high rare earth elements according to claim 7, characterized in that: The mixed acid solution comprises, by weight, 10 to 15 parts of acetic acid, 10 to 15 parts of anhydrous ethanol and 70 to 80 parts of water.

9. The method for thinning cover glass containing high rare earth elements according to claim 4, characterized in that: The temperature for chemical thinning is 45°C to 65°C.

10. A cover glass containing high rare earth elements, characterized in that: The thinning is carried out by the thinning method described in any one of claims 4 to 9.

Citation Information

Patent Citations

  • Liquid etchant and method for forming trench isolation structure using same

    CN102449746A

  • Etching solution for inhibiting pits after thinning of TFT liquid crystal display

    CN106186714A

  • Method for roughening surface using wet treatment

    CN108028194A

  • Etchant composition, method for forming wiring, and method for manufacturing array substrate for liquid crystal display device

    CN114075669A

  • Etching Composition

    US20150267112A1