Concrete corrosion and rust inhibitor and preparation method thereof

The composite anti-corrosion and rust inhibitor composed of kaolin and modified epoxy resin solves the problems of unreasonable formula and high cost in the existing technology, achieves high-efficiency anti-corrosion and rust-inhibition effect of concrete in various environments, and improves the Compression resistance and thermal stability.

CN118754501AInactive Publication Date: 2024-10-11WUHAN PINTAI NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410878526.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing anti-corrosion and rust-inhibiting agents for concrete have unreasonable formulas, unsatisfactory anti-corrosion and rust-inhibiting effects, some costs are high, and they perform poorly in various environments.

Method used

A composite anti-corrosion and rust inhibitor composed of kaolin, modified epoxy resin, silane coupling agent, nitrite, thiourea, sodium dodecyl sulfonate, sodium octyl sulfonate and shrinkage agent, through fine preparation Treatment and modification processes improve component dispersion and synergy to create a long-lasting corrosion barrier.

Benefits of technology

It significantly improves the sulfate resistance, chloride ion resistance and anti-permeability properties of concrete, enhances the compressive strength and thermal stability, reduces costs, and is suitable for a variety of environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004923833710000131
    Figure BDA0004923833710000131
Patent Text Reader

Abstract

The invention belongs to the technical field of building material additives, and particularly relates to a concrete corrosion and rust inhibitor and a preparation method thereof. The corrosion and rust inhibitor comprises the following components in percentage by weight: 3 to 5 percent of kaolin, 2 to 3 percent of modified epoxy resin, 1 to 3 percent of silane coupling agent, 5 to 10 percent of nitrite, 2 to 4 percent of thiourea, 6 to 10 percent of triethanolamine, 7 to 10 percent of sodium dodecyl sulfate, 1 to 5 percent of sodium octyl sulfonate, 15 to 20 percent of shrinking agent and the balance of water. The preparation method comprises the following steps: weighing the kaolin, the modified epoxy resin, the silane coupling agent, nitrite, thiourea, triethanolamine, sodium dodecyl sulfate, sodium octylsulfonate, the shrinking agent and water in percentage by mass, carrying out ultrasonic treatment at room temperature, standing, and stirring to obtain the concrete corrosion and rust inhibitor. The concrete anti-corrosion and anti-rust agent prepared by the preparation method disclosed by the invention not only has a composite characteristic, but also remarkably improves the durability of concrete in various environments through a unique preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of building material additives, and specifically relates to a concrete anticorrosion and rust inhibitor and a preparation method thereof. Background Art

[0002] With the rapid development of modern construction technology, concrete structures are increasingly used around the world. However, concrete structures are susceptible to corrosion during service, especially in environments containing corrosive media such as sulfate, magnesium, and chloride ions, which reduces the strength and durability of concrete structures and affects their service life. The main causes of common concrete reinforcement corrosion are: ① Concrete carbonization: Carbon dioxide in the air reacts with calcium hydroxide in concrete to form calcium carbonate, which reduces the alkalinity inside the concrete. When the carbonization depth reaches or exceeds the steel bar protective layer, the passivation film on the steel bar surface is destroyed, causing corrosion. ② Concrete quality: If the concrete water-cement ratio is too large, the amount of cement is insufficient, the vibration is not dense, or there are cracks, air, water, and carbon dioxide will easily invade, causing steel bar corrosion. ③ Chloride salt addition: Although chloride salt can enhance the early strength and antifreeze performance of concrete, excessive addition will destroy the passivation film on the steel bar surface and cause steel bar corrosion. Therefore, the specification stipulates the upper limit of chloride salt addition. ④ Corrosive gases: Acidic gases such as hydrogen chloride and chlorine are absorbed by concrete, which will reduce the alkalinity of concrete and cause steel bar corrosion. ⑤ Environmental humidity: Humidity has an important impact on steel corrosion. In very humid or very dry environments, steel corrosion is slow; under moderate humidity conditions, especially when the relative humidity is around 80%, the risk of steel corrosion is the highest. Therefore, it is necessary to develop a concrete anti-corrosion and rust inhibitor, which is a chemical substance that can effectively prevent or delay steel corrosion in concrete. It forms a protective film inside the concrete or on the surface of the steel bar to isolate the corrosive medium from the steel bar, thereby achieving the purpose of anti-corrosion and rust prevention.

[0003] Common types of concrete anti-corrosion and rust inhibitors:

[0004] Silicate preservative: Silicate preservative is an inorganic material that dissolves on the surface and turns the metal elements in concrete into insoluble compounds to achieve the purpose of corrosion prevention. Silicate preservatives have the effect of hardening concrete and increasing the strength of concrete, while also improving the durability and toughness of concrete. However, silicate preservatives are not suitable for co-firing pure basic concrete, and attention should be paid to the applicability of the material when using them.

[0005] Organic preservatives: Organic preservatives are composed of various organic compounds and have excellent permeability and chemical corrosion resistance. They can penetrate the metal inside the concrete and form a protective film to prevent it from contacting oxygen and moisture, thereby achieving an anti-corrosion effect. Organic preservatives are suitable for concrete structures with highly corrosive environments, such as chemical plants.

[0006] Composite concrete rust inhibitor: Composite concrete rust inhibitor is developed for sulfate and chloride corrosion. It increases the compactness of concrete by adding waterproofing agent and water reducing agent, and improves the concrete's resistance to the invasion of bad water quality; by adding high-performance sodium octyl sulfonate, it improves the freeze-thaw resistance and durability of concrete; through composite rust inhibitor, it obtains positive protection for steel bars and concrete after the invasion of bad water quality. This kind of anti-corrosion and rust inhibitor can fundamentally prevent or delay the corrosion of sulfate and chloride salts on concrete, and improve the durability of concrete. Therefore, many people are now starting to use composite concrete anti-corrosion and rust inhibitor. Therefore, many scholars have focused their research on composite concrete anti-corrosion and rust inhibitor.

[0007] The patent with announcement number CN110183136B discloses a concrete anticorrosion and rust inhibitor and its preparation method. The patent first prepares calcium nitrate solution and sodium carbonate aqueous solution separately, dissolves polycarboxylic acid water reducer and ethylenediaminetetramethylenephosphonic acid in water and places them in a four-necked flask, then adds calcium nitrate solution and sodium carbonate solution to the flask at a uniform speed, reacts at 20℃-35℃, and the whole dropping process is completed in 1-3h; dissolves barium nitrate, ethylene glycol, vitamin C, and disodium ethylenediaminetetraacetic acid in water, and puts them into nano calcium carbonate suspension and stirs them evenly. The concrete anticorrosion and rust inhibitor has good sulfate erosion resistance and rust prevention effect, and can achieve good concrete workability under low water-binder ratio, but due to the addition of vitamin C, the effect may be affected in high temperature and high humidity environment, and the durability of the anticorrosion and rust inhibitor needs to be further improved.

[0008] The patent with the announcement number CN117263565B discloses a multifunctional concrete anticorrosion and rust inhibitor and its preparation method. The multifunctional concrete anticorrosion and rust inhibitor disclosed in the patent includes 3.5-11 parts of corrosion inhibition components, 1-3 parts of waterproof components and 1-6 parts of densification components by weight; wherein the corrosion inhibition components include gluconate, nitrite and sodium isopropylbenzene sulfonate, the waterproof component includes one or more of sodium methyl silicate, sodium silicate and sodium metasilicate pentahydrate, and the densification component includes nano-silicon dioxide and / or organosilicon-nano calcium carbonate composite modified polypropylene. This technology can effectively resist the influence of chloride ions on the corrosion of concrete steel bars, and at the same time improve the ability of concrete to tolerate sulfate ions. However, the corrosion inhibition components gluconate, nitrite and sodium isopropylbenzene sulfonate are added in large amounts. Although the effect of corrosion prevention and rust prevention can be achieved, due to excessive dosage, from a long-term perspective, it may affect the service life of concrete. At the same time, the nanomaterials used are relatively expensive, which undoubtedly increases the cost of use.

[0009] Therefore, it is urgent to propose a concrete anti-corrosion and rust inhibitor with a more reasonable formula of components, better anti-corrosion and rust prevention effect, lower cost, and suitable for a variety of environments. Summary of the invention

[0010] In view of the problems of unreasonable formula, unsatisfactory anti-corrosion and rust inhibition effect, and high cost of some concrete anti-corrosion and rust inhibition agents in the prior art, the present application proposes a concrete anti-corrosion and rust inhibition agent and a preparation method thereof.

[0011] In a first aspect, the present application provides a concrete anti-corrosion and rust inhibitor, comprising the following components in weight percentage:

[0012] 3-5wt.% kaolin, 2-3wt.% modified epoxy resin, 1-3wt.% silane coupling agent, 5-10wt.% nitrite, 2-4wt.% thiourea, 6-10wt.% triethanolamine, 7-10wt.% sodium dodecyl sulfonate, 1-5wt.% sodium octyl sulfonate, 15-20wt.% shrinkage agent and the balance water.

[0013] In a specific embodiment, the kaolin needs to be pretreated before use, and the pretreatment method is:

[0014] Step S1. Pass kaolin through a 100-mesh sieve, then wash with water 1 to 2 times, filter and dry to obtain a solid sample a;

[0015] Step S2. calcining the solid sample a at 400-600° C. for 4-5 h, and then standing at room temperature to obtain a solid sample b;

[0016] Step S3. Mechanically ball-mill the solid sample b for 20 to 40 minutes, take it out and pass it through a 400-mesh sieve to obtain pretreated kaolin.

[0017] By adopting the above technical solution, after fine washing and calcination, the impurities and interlayer bound water in kaolin are effectively removed, which greatly improves its dispersibility in anti-corrosion and rust inhibitors. Based on its large specific surface area and strong adsorption capacity, kaolin can be tightly adsorbed between the layers or on the surface of the anti-corrosion and rust inhibitor. When it is added to concrete, it can slowly release the anti-corrosion and rust inhibitor to provide long-lasting anti-corrosion protection for concrete. At the same time, as a clay material, nano kaolin can also enhance the compressive strength of concrete, making it more durable.

[0018] In a specific embodiment, the treatment method of the modified epoxy resin is:

[0019] Step 1: Mix water and alginic acid, and stir at a temperature of 50 to 60° C. for 30 to 40 minutes to obtain a mixed system 1;

[0020] Step 2: adding epoxy resin and hydroxymethyl cellulose to the mixed system 1, stirring at a temperature of 50 to 60° C. for 1.5 to 3 hours to obtain a mixed system 2;

[0021] Step 3: Triethylenetetramine is added dropwise to the mixed system 2, and the mixture is stirred at 50-60° C. for 2-3 hours to obtain a mixed system 3, and the mixture is cooled to room temperature, filtered, washed, and dried to obtain a modified epoxy resin.

[0022] In a specific embodiment, the mass ratio of water: propylene glycol alginate epoxy resin: hydroxymethyl cellulose: triethylenetetramine is (40-50): (0.5-1): (25-35): (0.5-1): (3-5).

[0023] The modified epoxy resin glue obtained by adopting the above technical solution not only has excellent compressive strength and thermal stability, but also can play multiple roles in concrete. On the one hand, it can improve the compressive performance of concrete, enabling it to withstand greater external force impact; on the other hand, it can also enhance the thermal stability of concrete and reduce the risk of cracks and deformation caused by temperature changes. By introducing modified epoxy resin capsules, this application further expands the scope of use of concrete materials, enabling them to adapt to more complex environmental conditions.

[0024] In a specific embodiment, the silane coupling agent is one or more of trimethoxysilane, triethoxysilane and tri-n-propoxysilane.

[0025] In a specific embodiment, the nitrite is any one of calcium nitrite or sodium nitrite.

[0026] In a specific embodiment, the water reducing agent is any one of polycarboxylic acid or naphthalenesulfonic acid.

[0027] On the other hand, the present application provides a method for preparing a concrete anticorrosion and rust inhibitor, which is as follows:

[0028] First, kaolin, modified epoxy resin, silane coupling agent, nitrite, thiourea, triethanolamine, sodium dodecyl sulfonate, sodium octyl sulfonate, shrinking agent and water are weighed according to mass percentage, ultrasonically treated at room temperature for 20 to 40 minutes, then allowed to stand for 20 to 30 minutes, stirred at a speed of 90 to 120 r / min for 30 to 60 minutes at 45 to 50° C., to obtain a concrete anticorrosion and rust inhibitor.

[0029] In summary, the present application has the following beneficial effects: the concrete anticorrosion and rust inhibitor prepared in the present application not only has the characteristics of a composite concrete anticorrosion and rust inhibitor, but also significantly improves the concrete's resistance to sulfate, chloride ions, and impermeability in various environments through the preparation process of the present application. The details are as follows:

[0030] (1) The concrete anti-corrosion and rust inhibitor of the present application adopts a composite formula design, which integrates a variety of anti-corrosion and rust-inhibiting ingredients, so that the concrete can show stronger resistance to the corrosion of harmful substances such as sulfates and chloride ions. When this anti-corrosion and rust inhibitor is added to concrete, it can form a protective barrier inside the concrete, effectively blocking the penetration of these harmful substances, thereby significantly improving the concrete's resistance to sulfates, chloride ions, and impermeability.

[0031] (2) This application also introduces kaolin as an important component of the anti-corrosion and rust inhibitor. The pretreated kaolin obtained by fine water washing and calcination effectively removes impurities and interlayer bound water in the kaolin, which greatly improves its dispersibility in the anti-corrosion and rust inhibitor. Based on its large specific surface area and strong adsorption capacity, nano kaolin can be tightly adsorbed on the interlayer or surface of the anti-corrosion and rust inhibitor. When it is added to concrete, it can slowly release the anti-corrosion and rust inhibitor to provide long-lasting anti-corrosion protection for the concrete. At the same time, as a clay material, nano kaolin can also enhance the compressive strength of concrete, making it more durable.

[0032] (3) The present application modifies epoxy resin for use in concrete. This modified epoxy resin capsule not only has excellent compressive strength and thermal stability, but also plays multiple roles in concrete. On the one hand, it can improve the compressive properties of concrete, enabling it to withstand greater external force impacts; on the other hand, it can also enhance the thermal stability of concrete and reduce the risk of cracks and deformation caused by temperature changes. By introducing modified epoxy resin capsules, the present application further expands the scope of use of concrete materials, enabling them to adapt to more complex environmental conditions.

[0033] (4) Thiourea small molecule substances are also added to the concrete anticorrosion and rust inhibitor of the present application. Thiourea has strong water absorption performance and synergistic effect with the shrinkage agent, which can quickly remove water vapor in the concrete and prevent the interaction of water and other substances to cause steel corrosion. At the same time, thiourea can also interact with triethanolamine to fill the gaps in the cement, further improving the density and durability of the concrete.

[0034] (5) In order to improve the dispersibility of various substances in concrete, this application also introduces surfactants such as sodium dodecyl sulfonate, sodium octyl sulfonate and silane coupling agent. These surfactants can work synergistically with each other to promote the uniform distribution of anti-corrosion and rust inhibitors and other additives in concrete, ensuring that other additives can fully play their role. The concrete anti-corrosion and rust inhibitor of this application has shown good performance in improving the durability and corrosion resistance of concrete. DETAILED DESCRIPTION

[0035] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation method, structure, characteristics and effects of the present invention are described in detail below in combination with the preferred embodiments. It should be noted that the raw materials used in this application are all commercially available, among which kaolin is produced in Jiepai Town, Hengyang County, Hunan Province. After preliminary testing, the particle size distribution range of kaolin in this area is 1μm to 10μm, and the specific surface area is 10 to 50m 2 / g, specific gravity is 2.3~2.5g / cm 3 between.

[0036] Example 1

[0037] This embodiment provides a pretreatment method for kaolin, and the specific pretreatment method is as follows:

[0038] Step S1. Weigh 100 g of kaolin and pass it through a 100-mesh sieve to remove some impurities and large particles in the kaolin. Then put the sieved kaolin into 300 g of water, wash it twice, filter out the filtrate, and dry the solid in an oven at 100° C. for 5 hours to obtain a solid sample a1.

[0039] Step S2. The solid sample a1 is manually ground into powder to facilitate the removal of impurities and bound water in the kaolin, and the ground kaolin is placed in a muffle furnace for calcination at a heating rate of 25°C / min to 500°C for 4.5h, and then the muffle furnace is closed, and the sample is taken out at room temperature to obtain a solid sample b1;

[0040] Step S3. Put the solid sample b1 into a planetary ball mill, set the rotation speed to 240 r / min, ball mill for 30 min, take out the solid sample, and then pass it through a 400-mesh sieve to obtain a solid sample c1.

[0041] Example 2

[0042] This embodiment provides a pretreatment method for kaolin, and the specific pretreatment method is as follows:

[0043] Step S1. Weigh 100 g of kaolin and pass it through a 100-mesh sieve to remove some impurities and large particles in the kaolin. Then put the sieved kaolin into 300 g of water, wash it twice, filter out the filtrate, and dry the solid in an oven at 100° C. for 5 hours to obtain a solid sample a2;

[0044] Step S2. The solid sample a2 is manually ground into powder to facilitate the removal of impurities and bound water in the kaolin, and the ground kaolin is placed in a muffle furnace for calcination at a heating rate of 25°C / min to 400°C for calcination for 5h, and then the muffle furnace is closed, and the sample is taken out at room temperature to obtain a solid sample b2;

[0045] Step S3. Place the solid sample b2 into a planetary ball mill, set the rotation speed to 240 r / min, ball mill for 20 min, take out the solid sample, and then pass it through a 400-mesh sieve to obtain a solid sample c2.

[0046] Example 3

[0047] This embodiment provides a pretreatment method for kaolin, and the specific pretreatment method is as follows:

[0048] Step S1. Weigh 100 g of kaolin and pass it through a 100-mesh sieve to remove some impurities and large particles in the kaolin. Then put the sieved kaolin into 300 g of water, wash it twice, filter out the filtrate, and dry the solid in an oven at 100° C. for 5 hours to obtain a solid sample a3;

[0049] Step S2. The solid sample a3 is manually ground into powder to facilitate the removal of impurities and bound water in the kaolin, and the ground kaolin is placed in a muffle furnace for calcination at a heating rate of 25°C / min to 600°C for 4 hours, and then the muffle furnace is closed, and the sample is taken out at room temperature to obtain a solid sample b3;

[0050] Step S3. Place the solid sample b3 into a planetary ball mill, set the rotation speed to 240 r / min, ball mill for 40 min, take out the solid sample, and then pass it through a 400-mesh sieve to obtain a solid sample c3.

[0051] Comparative Example 1

[0052] The main difference between this comparative example and Example 1 is that the kaolin sample in this comparative example is not calcined in a muffle furnace to obtain sample c4.

[0053] Example 4

[0054] This embodiment provides a modification treatment method for epoxy resin, which is as follows:

[0055] Step 1: Mix water and alginic acid, stir magnetically for 35 min at a temperature of 55° C. and a rotation speed of 150 r / min to obtain a mixed system 1;

[0056] Step 2: adding epoxy resin and hydroxymethyl cellulose to the mixed system 1, and magnetically stirring at a temperature of 55° C. and a rotation speed of 150 r / min for 2.5 h to obtain a mixed system 2;

[0057] Step 3: Triethylenetetramine was added dropwise to the mixed system 2, and the mixture was stirred at 55°C for 2.5 hours to obtain a mixed system 3. The mixture was cooled to room temperature, the filtrate was removed, and the obtained solid was dried at 70°C for 5 hours to obtain a modified epoxy resin sample 1.

[0058] In the above embodiment, the mass ratio of water: alginic acid: propylene glycol ester epoxy resin: hydroxymethyl cellulose: triethylenetetramine is controlled to be 45:0.7:30:0.7:4.

[0059] Example 5

[0060] This embodiment provides a modification treatment method for epoxy resin, which is as follows:

[0061] Step 1: Mix water and alginic acid, stir magnetically for 40 min at a temperature of 50° C. and a rotation speed of 150 r / min to obtain a mixed system 1;

[0062] Step 2: adding epoxy resin and hydroxymethyl cellulose to the mixed system 1, and magnetically stirring at a temperature of 50° C. and a rotation speed of 150 r / min for 3 h to obtain a mixed system 2;

[0063] Step 3: Triethylenetetramine was added dropwise to the mixed system 2, and the mixture was stirred at 55°C for 2 hours to obtain a mixed system 3. The mixture was cooled to room temperature, the filtrate was removed, and the obtained solid was dried at 70°C for 5 hours to obtain a modified epoxy resin sample 1.

[0064] In the above embodiment, the mass ratio of water: alginic acid: propylene glycol ester epoxy resin: hydroxymethyl cellulose: triethylenetetramine is controlled to be 40:0.5:35:0.5:5.

[0065] Example 6

[0066] This embodiment provides a modification treatment method for epoxy resin, which is as follows:

[0067] Step 1: Mix water and alginic acid, stir magnetically for 30 min at 60°C and at a speed of 150 r / min to obtain a mixed system 1;

[0068] Step 2: adding epoxy resin and hydroxymethyl cellulose to the mixed system 1, and magnetically stirring at a temperature of 60° C. and a rotation speed of 150 r / min for 1.5 h to obtain a mixed system 2;

[0069] Step 3: Triethylenetetramine was added dropwise to the mixed system 2, and the mixture was stirred at 60°C for 3 hours to obtain a mixed system 3. The mixture was cooled to room temperature, the filtrate was removed, and the obtained solid was dried at 70°C for 5 hours to obtain a modified epoxy resin sample 1.

[0070] In the above embodiment, the mass ratio of water: alginic acid: propylene glycol ester epoxy resin: hydroxymethyl cellulose: triethylenetetramine is controlled to be 50:1:25:1:3.

[0071] Example 7

[0072] This embodiment provides a method for preparing a concrete anticorrosion and rust inhibitor, which is specifically as follows:

[0073] First, 4wt.% of kaolin prepared in Example 1, 4.5wt.% of modified epoxy resin prepared in Example 3, 2wt.% of trimethoxysilane, 7.5wt.% of calcium nitrite, 6wt.% of thiourea, 8wt.% of triethanolamine, 9wt.% of sodium dodecyl sulfate, 12wt.% of sodium octyl sulfate, 15wt.% of polycarboxylic acid and 32wt.% of water were weighed according to mass percentage, ultrasonically treated at room temperature for 30 min, then allowed to stand for 250 min, and stirred at 48°C at a speed of 110 r / min for 50 min to obtain a concrete anticorrosion and rust inhibitor.

[0074] Example 8

[0075] This embodiment provides a method for preparing a concrete anticorrosion and rust inhibitor, which is specifically as follows:

[0076] First, weigh 3wt.% kaolin prepared in Example 1, 6wt.% modified epoxy resin prepared in Example 5, 1wt.% triethoxysilane, 10wt.% calcium nitrite, 4wt.% thiourea, 10wt.% triethanolamine, 7wt.% sodium dodecyl sulfate, 15wt.% sodium octyl sulfate, 10wt.% polycarboxylic acid and 34wt.% water according to mass percentage, ultrasonically treat at room temperature for 30 minutes, then let stand for 25 minutes, and stir at 48°C at a speed of 110r / min for 50 minutes to obtain a concrete anti-corrosion and rust inhibitor.

[0077] Example 9

[0078] This embodiment provides a method for preparing a concrete anticorrosion and rust inhibitor, which is specifically as follows:

[0079] First, weigh 4.5wt.% kaolin prepared in Example 2, 5wt.% modified epoxy resin prepared in Example 5, 1.5wt.% tri-n-propoxysilane, 6wt.% calcium nitrite, 7wt.% thiourea, 7wt.% triethanolamine, 8wt.% sodium dodecylsulfonate, 11wt.% sodium octylsulfonate, 12wt.% naphthalenesulfonic acid and 38wt.% water according to mass percentage, ultrasonically treat at room temperature for 35min, then let stand for 22min, and stir at 46°C at a speed of 105r / min for 55min to obtain a concrete anti-corrosion and rust inhibitor.

[0080] Example 10

[0081] This embodiment provides a method for preparing a concrete anticorrosion and rust inhibitor, which is specifically as follows:

[0082] First, 5wt.% of kaolin prepared in Example 2, 3wt.% of modified epoxy resin prepared in Example 5, 3wt.% of triethoxysilane, 5wt.% of sodium nitrite, 8wt.% of thiourea, 6wt.% of triethanolamine, 10wt.% of sodium dodecylsulfonate, 10wt.% of sodium octylsulfonate, 20wt.% of naphthalenesulfonic acid and 30wt.% of water were weighed according to mass percentage, and ultrasonically treated at room temperature for 20min, then allowed to stand for 20min, and stirred at 50°C at a speed of 90r / min for 60min to obtain a concrete anticorrosion and rust inhibitor.

[0083] Embodiment 11

[0084] This embodiment provides a method for preparing a concrete anticorrosion and rust inhibitor, which is specifically as follows:

[0085] First, 3.5wt.% of kaolin prepared in Example 2, 5.5wt.% of modified epoxy resin prepared in Example 6, 2.5wt.% of tri-n-propoxysilane, 9wt.% of sodium nitrite, 5wt.% of thiourea, 9wt.% of triethanolamine, 8.5wt.% of sodium dodecylsulfonate, 13wt.% of sodium octylsulfonate, 18wt.% of polycarboxylic acid and 27wt.% of water were weighed by mass percentage, ultrasonically treated at room temperature for 40min, then allowed to stand for 30min, and stirred at 45°C at a speed of 120r / min for 30min to obtain a concrete anticorrosion and rust inhibitor.

[0086] Comparative Example 2

[0087] The main difference between this comparative example and Example 7 is that the kaolin sample used in this comparative example is the sample prepared in Comparative Example 1.

[0088] Comparative Example 3

[0089] The main difference between this comparative example and Example 7 is that the kaolin used in this comparative example has not been subjected to any treatment.

[0090] Comparative Example 4

[0091] The main difference between this comparative example and Example 7 is that the epoxy resin used in this comparative example has not been modified.

[0092] Comparative Example 5

[0093] The main difference between this comparative example and Example 7 is that no thiourea is added in this comparative example.

[0094] Performance Testing

[0095] Sulfate erosion coefficient ratio: The standard specimens at the age of 28 days are first immersed in 5% Na2SO4 solution for 15 hours, and then dried at 80±5℃ for 6 hours. The cycle test is carried out to determine the compressive strength of the concrete subjected to sulfate erosion. Then the ratio of the compressive strength of the control group and the blank group is calculated. The larger the ratio, the better the sulfate erosion resistance.

[0096] Chloride ion permeability coefficient ratio: It is the ratio of the chloride ion penetration depth between the 28-day-old samples in the control group and the blank group. The smaller the ratio, the better the resistance to chloride ion corrosion.

[0097] Anti-seepage grade: The anti-seepage performance is determined by the maximum water pressure that the sample at 28 days old can withstand during the test. The results are shown in Table 1.

[0098] Table 1

[0099]

[0100] Performance Analysis

[0101] By comparing the data in Table 1, it can be seen that the concrete anticorrosion and rust inhibitor prepared by the method proposed in this application has good sulfate resistance, chloride ion resistance and impermeability, among which Example 7 has the best effect, the sulfate erosion coefficient ratio is 160%, the chloride ion penetration coefficient ratio is 42 and the sample is free of rust, the 28-day compressive strength is 120, and the impermeability grade reaches P15. It may be that under this ratio, the components can cooperate with each other to achieve a good anticorrosion and rust-proof effect. On the one hand, it may be because the kaolin of this application is an important component of the anticorrosion and rust inhibitor. After fine washing and calcination treatment, the impurities and interlayer bound water in the kaolin are effectively removed, which greatly improves its dispersibility in the anticorrosion and rust inhibitor. Based on its large specific surface area and strong adsorption capacity, kaolin can be closely adsorbed on the interlayer or surface of the anticorrosion and rust inhibitor. When it is added to concrete, it can slowly release the anticorrosion and rust inhibitor, providing lasting anticorrosion protection for concrete. At the same time, as a clay material, nano kaolin can also enhance the compressive strength of concrete, making it more durable.

[0102] On the other hand, the modified epoxy resin prepared in this application can interact with many substances due to the high surface energy of the epoxy resin molecules, thereby improving the crosslinking density, mechanical strength and thermal stability of the epoxy resin. Therefore, the modified epoxy resin added to the anti-corrosion and rust inhibitor prepared in this application not only has excellent compressive strength and thermal stability, but also can play multiple roles in concrete. On the one hand, it can improve the compressive properties of concrete, enabling it to withstand greater external force impact; on the other hand, it can also enhance the thermal stability of concrete and reduce the risk of cracks and deformation caused by temperature changes. By introducing modified epoxy resin capsules, this application further expands the scope of use of concrete materials, enabling them to adapt to more complex environmental conditions.

[0103] In addition, the thiourea in the present application has a strong water absorption performance, and the synergistic effect with the shrinkage agent can quickly remove the water vapor in the concrete, and prevent the interaction of water with other substances to cause steel corrosion. At the same time, thiourea can also interact with triethanolamine to fill the gaps in the cement, further improving the density and durability of the concrete.

[0104] The surfactants added in this application include sodium dodecyl sulfonate, sodium octyl sulfonate and silane coupling agent. These surfactants can work together to promote the uniform distribution of anticorrosion and rust inhibitors and other additives in concrete, ensuring that other additives can fully play their role. The concrete anticorrosion and rust inhibitor of this application has shown good performance in improving the durability and corrosion resistance of concrete.

[0105] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A concrete anticorrosion and rust inhibitor, It is characterized in that The composition comprises the following weight percentages: 3-5wt.% kaolin, 2-3wt.% modified epoxy resin, 1-3wt.% silane coupling agent, 5-10wt.% nitrite, 2-4wt.% thiourea, 6-10wt.% triethanolamine, 7-10wt.% sodium dodecyl sulfonate, 1-5wt.% sodium octyl sulfonate, 15-20wt.% shrinkage agent and the balance water.

2. A concrete anticorrosion and rust inhibitor according to claim 1, It is characterized in that The kaolin needs to be pretreated before use, and the pretreatment method is: Step S1. Pass kaolin through a 100-mesh sieve, then wash with water 1 to 2 times, filter and dry to obtain a solid sample a; Step S2. calcining the solid sample a at 400-600° C. for 4-5 h, and then allowing to stand at room temperature to obtain a solid sample b; Step S3. Mechanically ball-mill the solid sample b for 20 to 40 minutes, take it out and pass it through a 400-mesh sieve to obtain pretreated kaolin.

3. A concrete anticorrosion and rust inhibitor according to claim 1, It is characterized in that The preparation method of the modified epoxy resin is: Step 1: Mix water and alginic acid, and stir at a temperature of 50 to 60° C. for 30 to 40 minutes to obtain a mixed system 1; Step 2: adding epoxy resin and hydroxymethyl cellulose to the mixed system 1, stirring at a temperature of 50 to 60° C. for 1.5 to 3 hours to obtain a mixed system 2; Step 3: Triethylenetetramine is added dropwise to the mixed system 2, and the mixture is stirred at 50-60° C. for 2-3 hours to obtain a mixed system 3, and the mixture is cooled to room temperature, filtered, washed, and dried to obtain a modified epoxy resin.

4. A concrete anticorrosion and rust inhibitor according to claim 3, It is characterized in that The mass ratio of water: propylene glycol alginate epoxy resin: hydroxymethyl cellulose: triethylenetetramine is (40-50): (0.5-1): (25-35): (0.5-1): (3-5).

5. A concrete anticorrosion and rust inhibitor according to claim 1, It is characterized in that The silane coupling agent is any one of trimethoxysilane, triethoxysilane and tri-n-propoxysilane.

6. A concrete anticorrosion and rust inhibitor according to claim 1, It is characterized in that The nitrite is any one of calcium nitrite or sodium nitrite.

7. A concrete anticorrosion and rust inhibitor according to claim 1, It is characterized in that The water reducing agent is any one of polycarboxylic acid or naphthalenesulfonic acid.

8. A method for preparing a concrete anticorrosion and rust inhibitor according to any one of claims 1 to 7, It is characterized in that The invention comprises the following components in parts by weight: firstly weigh kaolin, modified epoxy resin, silane coupling agent, nitrite, thiourea, triethanolamine, sodium dodecyl sulfonate, sodium octyl sulfonate, shrinking agent and water according to mass percentage, perform ultrasonic treatment at room temperature for 20 to 40 minutes, then stand for 20 to 30 minutes, stir at a speed of 90 to 120 r / min for 30 to 60 minutes at 45 to 50° C., and obtain a concrete anticorrosion and rust inhibitor.