Preparation method of steel slag self-healing recycled asphalt mixture

By introducing steel fiber and composite regenerant into the asphalt mixture, combined with microwave heating technology, the self-healing efficiency and durability of the asphalt mixture are improved, solving the problem of low self-healing rate in the existing technology, and extending the road use life.

CN118754512APending Publication Date: 2024-10-11SHENZHEN SEZ CONSTR GRP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411150825.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing self-healing asphalt mixture has a low self-healing rate and cannot effectively broaden its application range. As a result, the asphalt pavement is prone to cracking and aging in long-term use, affecting the durability and safety of the road.

Method used

The steel slag self-healing regenerated asphalt mixture preparation method is adopted. Steel fibers and composite regenerants are introduced into the asphalt, the component ratio and process flow are adjusted to improve the dynamic stability and high temperature stability of the mixture, and self-healing is promoted through microwave heating. combine.

Benefits of technology

It significantly improves the self-healing efficiency and road durability of the asphalt mixture, extends its service life, improves the asphalt colloid structure and rheological properties, and makes its performance close to that of new asphalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754512A_ABST
    Figure CN118754512A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a steel slag self-healing recycled asphalt mixture, and relates to the technical field of asphalt mixtures, and the preparation method comprises the following steps: (1) material preparation: weighing a recycled material rap, asphalt, aggregate, steel fiber, a composite regenerant and mineral powder; (2) preliminary mixing: sequentially adding the aggregate, the filler, the steel fiber and the composite regenerant into a stirrer, and uniformly stirring and mixing to obtain a mixed material; (3) preheating asphalt; and (4) mixing and compounding to obtain the required steel slag self-healing regenerated asphalt mixture. The steel fiber is introduced into the steel slag self-healing regenerated asphalt mixture, so that the dynamic stability of the mixture can be greatly improved, and the high-temperature stability of the steel slag self-healing regenerated asphalt mixture can be effectively improved; however, if the steel fiber is excessively doped, the dynamic stability of the steel slag self-healing regenerated asphalt mixture is reduced along with the great increase of the doping amount of the steel fiber, and the high-temperature stability is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of asphalt mixtures, and in particular to a method for preparing a steel slag self-healing regenerated asphalt mixture. Background Art

[0002] The construction of transportation infrastructure is the cornerstone of national development. As the process of urbanization continues to accelerate, the total mileage of highways continues to increase. Urban roads account for 1 / 3 of the total urban area. Therefore, the demand for highway construction continues to increase.

[0003] With the promulgation of the "Outline for Building a Strong Transportation Nation", building a strong transportation nation has become a major strategy for my country's current development.

[0004] Asphalt is a dark brown complex mixture of hydrocarbons of different molecular weights and their non-metallic derivatives. It is a kind of high-viscosity organic liquid, mostly in the form of liquid or semi-solid petroleum. It has a black surface and is soluble in carbon disulfide and carbon tetrachloride. Asphalt is an organic gelling material that is waterproof, moisture-proof and anti-corrosive. Therefore, asphalt can be widely used as a material for road paving. Due to its excellent performance, it is one of the most popular road paving materials.

[0005] However, there are also some problems with asphalt in actual use. For example, long-term exposure to the sun will cause asphalt aging and cracking, reducing its service life. In low temperature environments, asphalt is also prone to cracking and damage, affecting the durability and safety of the road. It can be seen that cracking is one of the more common forms of damage to asphalt pavements, and will seriously damage the bearing capacity of the pavement and shorten its service life over time.

[0006] Based on these problems, the use of self-healing asphalt mixture can greatly solve the problem of asphalt roadside cracking. However, the self-healing rate of the self-healing asphalt mixture in the prior art is low and its application range cannot be broadened.

[0007] Based on this, a method for preparing a steel slag self-healing recycled asphalt mixture is provided to solve the existing technical problems. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a steel slag self-healing regenerated asphalt mixture to solve the deficiencies in the prior art.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A method for preparing a steel slag self-healing regenerated asphalt mixture comprises the following steps:

[0011] (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight;

[0012] Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 10-40%, the mass fraction of aggregate is 20-55%, the mass fraction of steel fiber is 3-5%, the mass fraction of composite regeneration agent is 4-6%, the mass fraction of mineral powder is 1-1.5%, and the rest is asphalt;

[0013] (2) Preliminary mixing: adding aggregate, filler, steel fiber and composite regeneration agent to a mixer in sequence, stirring and mixing them evenly to obtain a mixed material;

[0014] Among them, the stirring and mixing speed is 350r / min;

[0015] (3) Asphalt preheating: Heat the asphalt to 170-180°C, keep warm and stir for 20 minutes to obtain preheated asphalt, and keep warm;

[0016] Among them, the speed of heat preservation and stirring is 400r / min;

[0017] (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 182-185° C., and stir for 15-20 min to obtain the desired steel slag self-healing recycled asphalt mixture;

[0018] Among them, the heat preservation stirring speed is 500r / min.

[0019] As a further technical solution, the preparation method of the composite regeneration agent in step (1) is:

[0020] First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil;

[0021] The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil:

[0022] Add rapeseed oil into the autoclave and pressurize it to 12-15 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate the air, maintain the pressure for 1 hour, and then discharge the material to complete the dehydration process;

[0023] Modifying castor oil to obtain modified castor oil;

[0024] Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 125-130°C, stir at 500r / min for 30-40min, then add auxiliary agent, adjust the temperature to 155-158°C, stir at 2000r / min for 20-30min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent;

[0025] The mixing mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 8-10:1-1.6:0.3-0.5:0.1-0.4.

[0026] As a further technical solution, the modified castor oil preparation method is:

[0027] Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil;

[0028] Among them, the vacuum drying temperature is 50°C and the time is 30min;

[0029] Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 85-90° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 102-105° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil;

[0030] The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 80-100:10-15:3-5;

[0031] The mass ratio of the dry castor oil to azobisisobutyronitrile is 10-12:1-1.5.

[0032] As a further technical solution, the inert gas is nitrogen or neon.

[0033] As a further technical solution, the plasticizer is epoxidized soybean oil.

[0034] As a further technical solution, the auxiliary agent is: 2-mercaptobenzimidazole aggregate is steel slag aggregate of different specifications.

[0035] As a further technical solution, the asphalt is: road petroleum asphalt 70#.

[0036] As a further technical solution, the apparent relative density of the mineral powder is 2.70.

[0037] As a further technical solution, the aggregate is steel slag;

[0038] The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are (12-15%), (30-35%), and (35-38%), and the remainder is 9-13mm specification steel slag aggregate.

[0039] As a further technical solution, the steel fiber has a diameter of 0.5 mm and a length of 50 mm.

[0040] The steel slag self-healing regenerated asphalt mixture of the present invention can promote self-healing by microwaves.

[0041] Beneficial effects:

[0042] The present invention can greatly improve the dynamic stability of the steel slag self-healing regenerated asphalt mixture by introducing steel fibers into the mixture, and can also effectively improve the high-temperature stability of the steel slag self-healing regenerated asphalt mixture; however, if excessive steel fibers are added, the dynamic stability of the steel slag self-healing regenerated asphalt mixture will decrease as the steel fiber dosage increases significantly, which will in turn cause a decrease in high-temperature stability and reduce the performance of the steel slag self-healing regenerated asphalt mixture. Therefore, the present invention can maximize the dynamic stability of the steel slag self-healing regenerated asphalt mixture by limiting the amount of steel fibers.

[0043] In the steel slag self-healing regenerated asphalt mixture of the present invention, by introducing a combination of multiple components, especially introducing the prepared composite regeneration agent, the healing properties of the composite regeneration agent can greatly improve the self-healing efficiency of the steel slag self-healing regenerated asphalt mixture, and the self-healing effect is good. The amount of each component added is determined according to the actual healing effect of the asphalt pavement, and the road durability is improved by improving the road self-healing efficiency, thereby extending the road service life.

[0044] The present invention introduces a certain amount of steel slag, which is a good microwave absorber, so that the steel slag has better heating performance under the action of microwaves. The present invention uses steel slag as aggregate and a special composite modified regeneration agent to prepare a steel slag self-healing regenerated asphalt mixture, which can better solve the compatibility problem between various components and further optimize the microwave heating effect of the steel slag self-healing regenerated asphalt mixture, thereby realizing efficient self-healing of the steel slag self-healing regenerated asphalt mixture.

[0045] In order to improve the regeneration performance of the asphalt mixture of the present invention, the present invention specially prepares a composite regeneration agent through a series of methods, which can improve and restore aged asphalt, adjust the viscosity of the system, and soften the rap so that it can be fully dispersed under the action of machinery and heating, so that the rap, asphalt and steel slag aggregate can be fully mixed and evenly mixed, thereby ensuring that the asphalt mixture has sufficient adhesion, and can promote the full blending of the rap and asphalt, and redissolve and disperse, which greatly improves the asphalt colloid structure, and then improves the rheological properties of the asphalt, so that the entire rap can recover or approach the performance of new asphalt. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 A flow chart of a method for preparing a steel slag self-healing recycled asphalt mixture;

[0047] Figure 2 It is a bar graph of effective heating depth of embodiments and comparative examples. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] The following are specific embodiments:

[0050] Example 1

[0051] A method for preparing a steel slag self-healing regenerated asphalt mixture comprises the following steps:

[0052] (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight;

[0053] Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 10%, the mass fraction of aggregate is 20%, the mass fraction of steel fiber is 3%, the mass fraction of composite regeneration agent is 4%, the mass fraction of mineral powder is 1%, and the rest is asphalt;

[0054] The preparation method of the composite regeneration agent is:

[0055] First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil;

[0056] The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil:

[0057] Add rapeseed oil into the autoclave, pressurize to 12 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate, maintain for 1 hour, and then discharge the material to complete the dehydration process;

[0058] Modifying castor oil to obtain modified castor oil;

[0059] Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 125°C, stir at 500r / min for 30min, then add auxiliary agent, adjust the temperature to 155°C, stir at 2000r / min for 20min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent;

[0060] The mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 8:1:0.3:0.1; the preparation method of the modified castor oil is:

[0061] Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil;

[0062] Among them, the vacuum drying temperature is 50°C and the time is 30min;

[0063] Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 85° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 102° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil;

[0064] The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 80:10:3;

[0065] The mass ratio of the dry castor oil to azobisisobutyronitrile is 10:1; the inert gas is nitrogen; the plasticizer is epoxy soybean oil; the auxiliary agent is: 2-mercaptobenzimidazole; the aggregate is steel slag aggregate of different specifications.

[0066] (2) Preliminary mixing: adding aggregate, filler, steel fiber and composite regeneration agent to a mixer in sequence, stirring and mixing them evenly to obtain a mixed material;

[0067] Among them, the stirring and mixing speed is 350r / min;

[0068] (3) Asphalt preheating: Heat the asphalt to 170°C, keep it warm and stir for 20 minutes to obtain preheated asphalt, and keep it warm;

[0069] Among them, the speed of heat preservation and stirring is 400r / min;

[0070] (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 182° C., and stir for 15 minutes to obtain the desired steel slag self-healing recycled asphalt mixture;

[0071] Among them, the heat preservation stirring speed is 500r / min.

[0072] Asphalt: road petroleum asphalt 70#.

[0073] The apparent relative density of the mineral powder is 2.70.

[0074] The aggregate is steel slag;

[0075] The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are 12%, 30%, and 35% respectively, and the remainder is 9-13mm specification steel slag aggregate.

[0076] The steel fiber has a diameter of 0.5 mm and a length of 50 mm.

[0077] Example 2

[0078] A method for preparing a steel slag self-healing regenerated asphalt mixture comprises the following steps:

[0079] (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight;

[0080] Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 20%, the mass fraction of aggregate is 32%, the mass fraction of steel fiber is 3.5%, the mass fraction of composite regeneration agent is 5%, the mass fraction of mineral powder is 1.2%, and the rest is asphalt;

[0081] The preparation method of the composite regeneration agent is:

[0082] First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil;

[0083] The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil:

[0084] Add rapeseed oil into the autoclave, pressurize to 13 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate, maintain for 1 hour, and then discharge the material to complete the dehydration process;

[0085] Modifying castor oil to obtain modified castor oil;

[0086] Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 128°C, stir at 500r / min for 35min, then add auxiliary agent, adjust the temperature to 156°C, stir at 2000r / min for 25min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent;

[0087] The mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 8.5:1.3:0.35:0.2; the preparation method of the modified castor oil is:

[0088] Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil;

[0089] Among them, the vacuum drying temperature is 50°C and the time is 30min;

[0090] Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 88° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 103° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil;

[0091] The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 85:12:3.5;

[0092] The mass ratio of the dry castor oil to azobisisobutyronitrile is 11:1.2; the inert gas is nitrogen; the plasticizer is epoxy soybean oil; the auxiliary agent is: 2-mercaptobenzimidazole; the aggregate is steel slag aggregate of different specifications.

[0093] (2) Preliminary mixing: adding aggregate, filler, steel fiber and composite regeneration agent to a mixer in sequence, stirring and mixing them evenly to obtain a mixed material;

[0094] Among them, the stirring and mixing speed is 350r / min;

[0095] (3) Asphalt preheating: Heat the asphalt to 175°C, keep it warm and stir for 20 minutes to obtain preheated asphalt, and keep it warm;

[0096] Among them, the speed of heat preservation and stirring is 400r / min;

[0097] (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 183° C., and stir for 18 minutes to obtain the desired steel slag self-healing recycled asphalt mixture;

[0098] Among them, the heat preservation stirring speed is 500r / min.

[0099] Asphalt: road petroleum asphalt 70#.

[0100] The apparent relative density of the mineral powder is 2.70.

[0101] The aggregate is steel slag;

[0102] The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are 13%, 33%, and 36% respectively, and the remainder is 9-13mm specification steel slag aggregate.

[0103] The steel fiber has a diameter of 0.5 mm and a length of 50 mm.

[0104] Example 3

[0105] A method for preparing a steel slag self-healing regenerated asphalt mixture comprises the following steps:

[0106] (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight;

[0107] Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 30%, the mass fraction of aggregate is 35%, the mass fraction of steel fiber is 4%, the mass fraction of composite regeneration agent is 5%, the mass fraction of mineral powder is 1.3%, and the rest is asphalt;

[0108] The preparation method of the composite regeneration agent is:

[0109] First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil;

[0110] The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil:

[0111] Add rapeseed oil into the autoclave, pressurize to 14 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate, maintain for 1 hour, and then discharge the material to complete the dehydration process;

[0112] Modifying castor oil to obtain modified castor oil;

[0113] Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 128°C, stir at 500r / min for 35min, then add auxiliary agent, adjust the temperature to 156°C, stir at 2000r / min for 25min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent;

[0114] The mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 9:1.5:0.4:0.3; the preparation method of the modified castor oil is:

[0115] Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil;

[0116] Among them, the vacuum drying temperature is 50°C and the time is 30min;

[0117] Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 88° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 104° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil;

[0118] The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 90:14:4;

[0119] The mass ratio of the dry castor oil to azobisisobutyronitrile is 11:1.2; the inert gas is nitrogen; the plasticizer is epoxy soybean oil; the auxiliary agent is: 2-mercaptobenzimidazole; the aggregate is steel slag aggregate of different specifications.

[0120] (2) Preliminary mixing: adding aggregate, filler, steel fiber and composite regeneration agent to a mixer in sequence, stirring and mixing them evenly to obtain a mixed material;

[0121] Among them, the stirring and mixing speed is 350r / min;

[0122] (3) Asphalt preheating: Heat the asphalt to 178°C, keep it warm and stir for 20 minutes to obtain preheated asphalt, and keep it warm;

[0123] Among them, the speed of heat preservation and stirring is 400r / min;

[0124] (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 183° C., and stir for 18 minutes to obtain the desired steel slag self-healing recycled asphalt mixture;

[0125] Among them, the heat preservation stirring speed is 500r / min.

[0126] Asphalt: road petroleum asphalt 70#.

[0127] The apparent relative density of the mineral powder is 2.70.

[0128] The aggregate is steel slag;

[0129] The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are 14%, 32%, and 37% respectively, and the remainder is 9-13mm specification steel slag aggregate.

[0130] The steel fiber has a diameter of 0.5 mm and a length of 50 mm.

[0131] Example 4

[0132] A method for preparing a steel slag self-healing regenerated asphalt mixture comprises the following steps:

[0133] (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight;

[0134] Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 40%, the mass fraction of aggregate is 25%, the mass fraction of steel fiber is 5%, the mass fraction of composite regeneration agent is 6%, the mass fraction of mineral powder is 1.5%, and the rest is asphalt;

[0135] The preparation method of the composite regeneration agent is:

[0136] First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil;

[0137] The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil:

[0138] Add rapeseed oil into the autoclave, pressurize to 15 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate, maintain for 1 hour, and then discharge the material to complete the dehydration process;

[0139] Modifying castor oil to obtain modified castor oil;

[0140] Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 130°C, stir at 500r / min for 40min, then add auxiliary agent, adjust the temperature to 158°C, stir at 2000r / min for 30min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent;

[0141] The mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 10:1.6:0.5:0.4; the preparation method of the modified castor oil is:

[0142] Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil;

[0143] Among them, the vacuum drying temperature is 50°C and the time is 30min;

[0144] Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 90° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 105° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil;

[0145] The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 100:15:5;

[0146] The mass ratio of the dry castor oil to azobisisobutyronitrile is 12:1.5; the inert gas is nitrogen; the plasticizer is epoxy soybean oil; the auxiliary agent is 2-mercaptobenzimidazole; and the aggregates are steel slag aggregates of different specifications.

[0147] (2) Preliminary mixing: adding aggregate, filler, steel fiber and composite regeneration agent to a mixer in sequence, stirring and mixing them evenly to obtain a mixed material;

[0148] Among them, the stirring and mixing speed is 350r / min;

[0149] (3) Asphalt preheating: Heat the asphalt to 180°C, keep it warm and stir for 20 minutes to obtain preheated asphalt, and keep it warm;

[0150] Among them, the speed of heat preservation and stirring is 400r / min;

[0151] (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 185° C., and stir for 20 minutes to obtain the desired steel slag self-healing recycled asphalt mixture;

[0152] Among them, the heat preservation stirring speed is 500r / min.

[0153] Asphalt: road petroleum asphalt 70#.

[0154] The apparent relative density of the mineral powder is 2.70.

[0155] The aggregate is steel slag;

[0156] The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are 15%, 35%, and 38% respectively, and the remainder is 9-13mm specification steel slag aggregate.

[0157] The steel fiber has a diameter of 0.5 mm and a length of 50 mm.

[0158] Comparative Example 1:

[0159] On the basis of Example 1, in the preparation process of the composite modifier, the modified castor oil is replaced by castor oil, and the remaining technical schemes are as follows.

[0160] Comparative Example 2:

[0161] On the basis of Example 1, no modified castor oil is added during the preparation of the composite modifier, and the remaining technical schemes are as follows.

[0162] test:

[0163] Test method for self-healing performance of steel slag asphalt mixture

[0164] The examples and comparative samples were tested:

[0165] An electromagnetic induction heater and an infrared camera were used to induction heat the recycled asphalt mixture. The voltage and output power were 650V and 7.9 kW, respectively. The heating distance was 10mm (coil to Marshall sample surface), and the heating time increased from 20 seconds to 100 seconds with an interval of 20 seconds. The average temperature of the Marshall specimen surface was collected using FLIR tool software. The induction heating efficiency was evaluated by performing induced temperature rise (IT I) on samples with different heating times.

[0166] The effective heating depth (EHD) accurately reflects the effective range of induction heating on the sample, and its calculation method is shown in formula (1).

[0167]

[0168] In the above formula, hs is the height of the rectangle where the average temperature reaches the softening point of the asphalt in the infrared image, hm is the height of the Marshall sample in the infrared image, and H is the actual height of the corresponding Marshall sample.

[0169] Table 1

[0170] Effective heating depth (EHD) cm Example 1 8.3 Example 2 8.6 Example 3 8.2 Example 4 8.1 Comparative Example 1 5.9 Comparative Example 2 4.6

[0171] It can be seen from Table 1 that the steel slag self-healing regenerated asphalt mixture prepared by the present invention has a deeper effective heating depth.

[0172] In order to simulate the fracture failure process of stamping parts, three-point bending tests were carried out on semicircular bending specimens. The maximum force of the specimen was obtained using a universal testing machine (UTM-25). The SCB specimens were pretreated in a temperature box at -10°C for 4 hours to achieve brittle failure. The loading rate was 0.5mm / min. Four parallel samples were used for the fracture healing (1 cycle) test. A total of five cycles were performed to measure multiple healing characteristics.

[0173] Two healing indices (strength healing rate and fracture energy healing rate) are selected to evaluate the healing performance of recycled asphalt mixture. The strength healing rate (HRS) is calculated by the failure load before and after healing, as shown in formula (2).

[0174]

[0175] Where Fh and F0 represent the critical load after healing and the initial critical load at fracture. The calculation formula of fracture energy (E) is shown in formula (3-5).

[0176]

[0177] Where E represents the fracture energy (J / m2), Wf represents the fracture work (J), Al ig represents the ligament area (m2), r, a and t represent the radius (m), notch length (m) and sample thickness (m). The fracture energy healing rate (HRE) is defined as the ratio of the fracture energy after healing (Eh) to the initial fracture energy (E0), which can be obtained according to formula (6).

[0178]

[0179] Table 2

[0180] Strength healing rate % Fracture energy healing rate % Example 1 81.3 95.4 Example 2 83.3 96.0 Example 3 82.9 95.7 Example 4 82.2 95.3 Comparative Example 1 69.5 78.2 Comparative Example 2 58.1 67.7

[0181] It can be seen from Table 2 that the asphalt mixture of the present invention has high self-healing performance.

[0182] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A method for preparing a steel slag self-healing recycled asphalt mixture, characterized in that: The following steps are involved: (1) Material preparation: Weigh the recycled material rap, asphalt, aggregate, steel fiber, composite regeneration agent, and mineral powder respectively according to weight; Among them, based on the total amount of steel slag self-healing recycled asphalt mixture, the mass fraction of recycled material rap is 10-40%, the mass fraction of aggregate is 20-55%, the mass fraction of steel fiber is 3-5%, the mass fraction of composite regeneration agent is 4-6%, the mass fraction of mineral powder is 1-1.5%, and the rest is asphalt; (2) Preliminary mixing: Add aggregate, filler, steel fiber and composite regeneration agent into a mixer in sequence, stir and mix them evenly to obtain a mixed material; Among them, the stirring and mixing speed is 350r / min; (3) Asphalt preheating: Heat the asphalt to 170-180°C, keep warm and stir for 20 minutes to obtain preheated asphalt, and keep warm; Among them, the speed of heat preservation and stirring is 400r / min; (4) Compounding: Add the mixture obtained in step (2) to the heated asphalt, adjust the temperature to 182-185°C, and stir for 15-20 minutes to obtain the desired steel slag self-healing recycled asphalt mixture; Among them, the heat preservation stirring speed is 500r / min.

2. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The preparation method of the composite regeneration agent in step (1) is: First, the rapeseed oil and castor oil are filtered to remove impurities in the rapeseed oil and castor oil; The rapeseed oil is dehydrated to obtain dehydrated rapeseed oil: Add rapeseed oil into the autoclave and pressurize it to 12-15 MPa, adjust the temperature to 100°C, maintain the pressure for 10 minutes, then release the pressure, evacuate the air, maintain the pressure for 1 hour, and then discharge the material to complete the dehydration process; Modifying castor oil to obtain modified castor oil; Add rapeseed oil, modified castor oil and plasticizer into a vacuum reactor in sequence, adjust the temperature to 125-130°C, stir at 500r / min for 30-40min, then add auxiliary agent, adjust the temperature to 155-158°C, stir at 2000r / min for 20-30min, discharge, and cool naturally to room temperature to obtain a composite regeneration agent; The mixing mass ratio of the rapeseed oil, modified castor oil, plasticizer and additive is 8-10:1-1.6:0.3-0.5:0.1-0.

4.

3. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 2, characterized in that: The modified castor oil preparation method is: Firstly, the castor oil is subjected to vacuum drying to obtain dry castor oil; Among them, the vacuum drying temperature is 50°C and the time is 30min; Then, dry castor oil, mercaptoethanol, and trimethylolpropane oleate are added into the reactor in sequence, and then an inert gas is introduced into the reactor, and the air in the reactor is exhausted, and then azobisisobutyronitrile is added, and the temperature is adjusted to 85-90° C., and stirred for reaction for 2 hours, and then the temperature is adjusted to 102-105° C., and stirring is continued for 2 hours. After cooling to room temperature, ethyl acetate is added to collect the reaction product, and the reaction product is washed with water and dried by rotary evaporation to obtain modified castor oil; The mixed mass ratio of the dry castor oil, mercaptoethanol and trimethylolpropane oleate is 80-100:10-15:3-5; The mass ratio of the dry castor oil to azobisisobutyronitrile is 10-12:1-1.

5.

4. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 3, characterized in that: The inert gas is nitrogen or neon.

5. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 2, characterized in that: The plasticizer is epoxidized soybean oil.

6. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The auxiliary agent is: 2-mercaptobenzimidazole. The aggregate is steel slag aggregate of different specifications.

7. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The asphalt is: road petroleum asphalt 70#.

8. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The apparent relative density of the mineral powder is 2.

70.

9. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The aggregate is steel slag; The specifications of the steel slag aggregate include 0-3mm, 3-5mm, 5-8mm, and 9-13mm, and the proportions of each specification are (12-15%), (30-35%), and (35-38%) respectively, and the remainder is 9-13mm specification steel slag aggregate.

10. The method for preparing a steel slag self-healing regenerated asphalt mixture according to claim 1, characterized in that: The steel fiber has a diameter of 0.5 mm and a length of 50 mm.

Citation Information

Patent Citations

  • Aged asphalt regenerant and preparation method thereof

    CN110982290A

  • Novel super-hydrophobic oil-absorbing porous degradable material

    CN117482906A