Lithium slag-based geopolymer filling material as well as preparation method and application thereof

Through the preparation of lithium slag-based polymer filling materials, combined with the specific formula and process of lithium slag, fly ash, slag, phosphogypsum and other components, the multiple performance problems of lithium slag composite materials have been solved, and high strength and low secretion have been achieved. Water rate and corrosion resistance meet the high standard requirements of building materials, realizing resource utilization and environmental protection of lithium slag.

CN118754530APending Publication Date: 2024-10-11GUIZHOU DEEP CARBON TECH CO LTD +1

Patent Information

Application Number
CN202410962166.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult for the existing technology to simultaneously meet the heavy metal leaching, sulfate corrosion resistance, fluidity and high mechanical properties of lithium slag composite materials, making it difficult to achieve resource utilization and environmental protection after lithium slag treatment.

Method used

By preparing lithium slag-based polymer filling materials, specific formulas and processes are adopted, including a combination of lithium slag, fly ash, slag, phosphogypsum, yellow phosphorus slag, zeolite and activators, and the materials are improved through alkali excitation and physical activation. activity, optimizing component proportions and particle sizes to form composite materials with high strength, low bleeding rate, and corrosion resistance.

Benefits of technology

It achieves high strength, suitable fluidity, low heavy metal leaching and resistance to sulfate erosion of lithium slag-based composite materials, meets the construction and environmental protection requirements of building materials, and realizes resource utilization and environmental protection of lithium slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004950587460000051
    Figure BDA0004950587460000051
  • Figure BDA0004950587460000061
    Figure BDA0004950587460000061
  • Figure BDA0004950587460000071
    Figure BDA0004950587460000071
Patent Text Reader

Abstract

The invention discloses a lithium slag based geopolymer filling material and a preparation method and application thereof, the lithium slag based geopolymer filling material comprises the following components in parts by weight: 30-60 parts of lithium slag, 10-20 parts of fly ash, 10-30 parts of slag, 10-25 parts of phosphogypsum, 5-10 parts of zeolite, 5-20 parts of yellow phosphorus slag, 5-10 parts of an exciting agent, 0.25-0.75 part of an additive and 35-50 parts of water, the mass ratio of the ardealite to the yellow phosphorus slag is (0.7-3.7): 1, and the exciting agent is sodium metasilicate and caustic soda. The lithium slag-based geopolymer filling material disclosed by the invention has the advantages of high strength, high sulfuric acid corrosion resistance, low bleeding rate and excellent flowability while meeting the requirements of heavy metal leaching concentration and low radioactivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a lithium slag-based polymer filling material and a preparation method and application thereof. Background Art

[0002] In recent years, with the rapid development of new energy vehicles and lithium electronic products, the demand for lithium has increased significantly, and the corresponding industrial waste lithium slag produced by the industrial lithium extraction industry has also increased year by year. Generally, 8 to 10 tons of lithium slag will be produced for every 1t of lithium salt produced. It is calculated that the annual discharge of lithium slag reaches more than 1.25 million tons. In addition to the accumulated amount over the years, the domestic lithium slag stockpile can reach tens of millions of tons. The accumulation of lithium slag will cause a lot of land waste and environmental pollution. The discharge of lithium slag will also cause the leaching of heavy metals such as cadmium, thallium, and lead. In order to avoid resource waste and reduce the harm caused by lithium slag as much as possible, harmless treatment and resource utilization of lithium slag are the current research hotspots. Because it is difficult to take into account the heavy metal leaching, sulfate corrosion resistance, fluidity and high mechanical properties of lithium slag composite materials at the same time after the treatment of lithium slag in the current technology. Therefore, it is urgent to develop a composite material that can meet the heavy metal leaching standards, high fluidity, high strength and corrosion resistance while absorbing lithium slag. Summary of the invention

[0003] In view of the defects in the prior art, the present invention proposes a lithium slag-based polymer filling material and a preparation method and application thereof.

[0004] The invention provides a lithium slag-based polymer filling material, which comprises the following components by weight: 30-60 parts of lithium slag, such as 30, 35, 40, 45, 50, 55, 60 parts; 10-20 parts of fly ash, such as 10, 12, 14, 16, 18, 20 parts; 10-30 parts of slag, such as 10, 15, 20, 25, 30 parts; 10-25 parts of phosphogypsum, such as 10, 12, 14, 16, 18, 20, 22, 25 parts; 5-10 parts of zeolite, such as 5, 6, 7, 8, 9, 10 parts; 5-20 parts of yellow phosphorus slag, such as 5, 8, 10, 12, 1 4, 16, 18, 20 parts; activator 5-10 parts, such as 5, 6, 7, 8, 9, 10 parts; admixture 0.25-0.75 parts, such as 0.25, 0.35, 0.45, 0.5, 0.6, 0.7, 0.75 parts; water 35-50 parts, such as 35, 40, 45, 50 parts; wherein the mass ratio of the phosphogypsum to the yellow phosphorus slag is (0.7-3.7): 1, such as 0.7:1, 0.75:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 3.7:1, and the activator is sodium metasilicate and caustic soda.

[0005] Since lithium slag contains a certain amount of SiO2 and Al2O3, the activity of lithium slag can be improved through alkali excitation, and then through specific formula and proportion adjustment, it can be prepared into lithium slag-based geological filling material, realizing the resource utilization of lithium slag while meeting various material properties.

[0006] In order to absorb more solid waste, the present application also rationally matches the formula through the interaction between the components, so as to realize the simultaneous absorption of solid wastes such as lithium slag, fly ash, phosphogypsum, slag and yellow phosphorus slag. At the same time, through the stimulating effect of phosphogypsum on yellow phosphorus slag, the ratio between phosphogypsum and yellow phosphorus slag is screened, which significantly improves the early strength of the material and obtains a composite material that can meet multiple performance requirements.

[0007] Furthermore, the specific surface area of ​​the lithium slag is 400-600 kg / m 3 The specific surface area of ​​lithium slag is obtained by drying at 100-110℃ for 22-24h, cooling to room temperature, and ball milling in a ball mill at 300-350r / min for 10-30min. By crushing coarse particles to increase the specific surface area, the particle grading can be improved, the surface dense structure of the glass body can be destroyed, the internal SiO2 and Al2O3 can be dissolved, and the activity of lithium slag can be improved. The specific surface area is tested by GB / T 8074-2008 "Determination of Specific Surface Area of ​​Cement" Blaine method.

[0008] Furthermore, the specific surface area of ​​the fly ash is 300-500 kg / m 3 The fly ash with a specific surface area is dried at 100-110℃ for 2-4h, cooled to room temperature, and milled in a ball mill at 300-350r / min for 30-60min. The specific surface area is tested according to GB / T 8074-2008 "Determination of Specific Surface Area of ​​Cement - Blaine Method". Fly ash is also physically activated to increase the specific surface area by crushing coarse particles to improve particle grading, destroy the dense surface structure of the glass body, and dissolve the internal SiO2 and Al2O3.

[0009] Furthermore, the specific surface area of ​​the slag is 450-550 kg / m 3 The slag with a specific surface area is dried at 100-110℃ for 4-12h, cooled to room temperature, ground in a vertical mill for 280-380min, and then ground in a ball mill for 10-40min. The specific surface area is tested according to GB / T 8074-2008 "Determination of Specific Surface Area of ​​Cement - Blaine Method". In order to ensure that the slag has high activity, slag powder with a 28-day activity index that meets the S105 grade standard is used, and the activity index is tested according to GB / T 18046-2017.

[0010] Furthermore, the mass ratio of the phosphogypsum to the yellow phosphorus slag is (2-3):1.

[0011] Furthermore, the admixture is at least one of sodium lignin sulfonate, naphthalene-based water reducer or polycarboxylic acid-based water reducer, preferably at least one of sodium lignin sulfonate or naphthalene-based water reducer.

[0012] Furthermore, the admixture is prepared by mixing sodium lignin sulfonate and naphthalene-based water reducer in a mass ratio of (0.5-1.5):1.

[0013] Further, the zeolite is a natural zeolite with a particle size of 28-74 μm, such as 28, 30, 35, 40, 46, 48, 50, 55, 60, 65, 70, 74 μm. Natural zeolite contains a large amount of Al2O3 and SiO2, and is composed of a three-dimensional framework of silicon-oxygen and aluminum-oxygen tetrahedrons, with a high porosity and cavity network and a strong ion exchange capacity. The finer the zeolite, the higher the reaction activity, the more hydration products at the same age, and the faster the reaction. However, the zeolite particle size is too small, and the water absorption rate will increase, which is easy to cause water bleeding of the filling material and affect the mechanical properties of the material. The preferred zeolite particle size is 48-74 μm. The specific particle size of the zeolite is obtained by drying and then ball milling, and ball milling can also improve its sphericity.

[0014] Furthermore, the specific surface area of ​​the yellow phosphorus slag is 450-550m 2 / kg, yellow phosphorus slag with a specific specific surface area is dried at 100-110℃ for 4-12h, cooled to room temperature, ground in a vertical mill for 240-360min, and then ground in a ball mill for 30-60min to obtain the specific surface area. The specific surface area is tested by GB / T 8074-2008 "Determination of Specific Surface Area of ​​Cement" Blaine method. Yellow phosphorus slag can generate C-(A)-SH gel by activating agent, but the Al2O3 content in yellow phosphorus slag is relatively low. After adding phosphogypsum, under the action of specific activators, it can better exert its potential activity and improve its hydration degree.

[0015] Furthermore, the phosphogypsum mainly plays a retarding role in the system and also plays a role in stimulating the activity of yellow phosphorus slag. It can be dried to a semi-hydrated gypsum state and then ground and crushed by a ball mill.

[0016] The present application also provides a method for preparing the lithium slag-based polymer filling material, comprising the following steps:

[0017] Weigh lithium slag, fly ash, slag, phosphogypsum, zeolite, yellow phosphorus slag, activator, admixture and water by weight, stir and mix evenly according to the experimental steps of "Test Method for Strength of Cement Mortar (ISO Method)" GB / T17671-2021, and then shape them to obtain a lithium slag-based polymer filling material.

[0018] The present application also provides the use of the lithium slag-based polymer filling material as a grouting material in construction engineering.

[0019] Unless otherwise specified, the specific surface area in this application refers to the specific surface area of ​​the raw material spherical model.

[0020] In summary, compared with the prior art, the present invention achieves the following technical effects:

[0021] (1) The lithium slag-based polymer filling material provided by the present invention has high strength;

[0022] (2) The lithium slag-based polymer filling material provided by the present invention has suitable fluidity and is easy to construct;

[0023] (3) The lithium slag-based polymer filling material provided by the present invention simultaneously solves the problem of heavy metal leaching and radioactivity of lithium slag solid waste;

[0024] (4) The lithium slag-based polymer filling material provided by the present invention can resist sulfate corrosion;

[0025] (5) The lithium slag-based polymer filling material provided by the present invention has a low water bleeding rate;

[0026] (6) The present invention realizes resource utilization of solid waste by a simple and low-cost method, thus meeting environmental protection requirements. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] Example

[0029] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following examples, and are particularly not limited to the types of the various component raw materials used in the following specific examples.

[0030] 1. The sources of raw materials for the embodiments and comparative examples are as follows:

[0031] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available, and different particle sizes of the same raw material are obtained by ball milling. The specific raw materials are selected as follows:

[0032]

[0033] The preparation method of the lithium slag-based polymer filling material of the embodiment of the present invention and the comparative example comprises the following steps:

[0034] Lithium slag, fly ash, slag, phosphogypsum, zeolite and yellow phosphorus slag are weighed by weight, dried and then ball-milled, stirred and mixed, an activator is added, and then an admixture and water are added to obtain a filling material.

[0035] 2. Various performance test methods

[0036] (1) Strength test: Tested according to "Test method for strength of cement mortar (ISO method)" GB / T17671-2021.

[0037] (2) Fluidity test: The test is carried out in accordance with the "Method for Determination of Fluidity of Cement Mortar" GB / T2419-2005.

[0038] (3) Heavy metal leaching concentration test: Tested in accordance with "Determination of Metal Elements in Solid Waste by Inductively Coupled Plasma Mass Spectrometry" HJ766-2015.

[0039] (4) Sulfate corrosion resistance test: The test is carried out according to the "Test method for sulfate corrosion resistance of cement" GB / T749-2008.

[0040] (5) Radioactivity test: Test in accordance with the Limits of Radioactive Nuclides in Building Materials GB 6566-2010.

[0041] (6) Water seepage rate test: The test shall be conducted in accordance with the Standard for Test Methods for Performance of Ordinary Concrete Mixtures GB T50080-2016.

[0042] Table 1 Technical solution of the embodiment (unit is weight part)

[0043]

[0044]

[0045] Table 2 Comparative Example Technical Scheme (Units are parts by weight)

[0046]

[0047]

[0048] Table 3. Effect data of examples and comparative examples

[0049]

[0050] Table 3. Effect data of examples and comparative examples

[0051]

[0052]

[0053] In Examples 1-11, multiple solid wastes such as lithium slag, fly ash, slag, and phosphogypsum are added at the same time, and by exploring the formula and optimizing the component ratio, the prepared composite material can meet multiple performances at the same time. First, the prepared material has high strength, the 3d flexural strength reaches 3Mpa or above, the compressive strength reaches 6MPa or above, generally higher than 7MPa, the 28d flexural strength reaches 5.5MPa or above, the compressive strength reaches 11.2MPa or above, generally higher than 13MPa; secondly, the material has good fluidity and strong processability; and the water bleeding rate of the material is low, which can meet the standard requirements for filling materials; the prepared lithium slag-based composite material simultaneously solves the problems of heavy metal leaching and radioactivity of lithium slag, both of which are within the range specified by the standard; the material also has excellent resistance to sulfuric acid corrosion, can be used in various environments, and has strong adaptability.

[0054] Comparative Examples 1-4 are all compared with Example 6. Comparative Example 1 only adds one activator, Comparative Example 2 has a mass ratio of phosphogypsum to yellow phosphorus slag that is not within the range, Comparative Example 3 has too much phosphogypsum added, and Comparative Example 4 does not contain zeolite in the system. The above comparative examples cannot meet the requirements of having low heavy metal leaching concentration and radioactivity while also having high strength, high resistance to sulfuric acid erosion, excellent fluidity and even strong processability.

[0055] Based on the test data of flexural strength, compressive strength, fluidity, sulfuric acid corrosion resistance, radioactivity and heavy metal leaching concentration of the filling material in Table 3, the lithium slag-based polymer filling material prepared by Examples 1-11 has obvious advantages over the comparative example and can effectively meet the high standards of customers and the market.

[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A lithium slag-based polymer filling material, characterized in that: By weight, it includes the following components: The mass ratio of the phosphogypsum to the yellow phosphorus slag is (0.7-3.7):1, and the activators are sodium metasilicate and caustic soda.

2. The lithium slag-based polymer filling material according to claim 1, characterized in that: The specific surface area of ​​the lithium slag is 400-600 kg / m 3 .

3. The lithium slag-based polymer filling material according to claim 1, characterized in that: The specific surface area of ​​the fly ash is 300-500kg / m 3 .

4. The lithium slag-based polymer filling material according to claim 1, characterized in that: The specific surface area of ​​the slag is 450-550 kg / m 3 .

5. The lithium slag-based polymer filling material according to claim 1, characterized in that: The mass ratio of the phosphogypsum to the yellow phosphorus slag is (2-3):

1.

6. The lithium slag-based polymer filling material according to claim 1, characterized in that: The additive is any one of sodium lignin sulfonate or naphthalene-based water reducer or a mixture of the two.

7. The lithium slag-based polymer filling material according to claim 1, characterized in that: The particle size of the zeolite is 48-74 μm.

8. The lithium slag-based polymer filling material according to claim 1, characterized in that: The specific surface area of ​​the yellow phosphorus slag is 450-550 kg / m 3 .

9. The method for preparing the lithium slag-based polymer filling material according to any one of claims 1 to 8, characterized in that: The steps include: Lithium slag, fly ash, slag, phosphogypsum, zeolite, yellow phosphorus slag, activator, additive and water are weighed in parts by weight, stirred and mixed evenly and then formed to obtain a lithium slag-based polymer filling material.

10. Use of the lithium slag-based polymer filling material according to any one of claims 1 to 8 as a grouting material in construction engineering.

Citation Information

Patent Citations

  • Mixed material for filling mine roadway

    CN102910888A

  • Geopolymer injecting paste material and preparing method and application thereof

    CN105541140A

  • Large-volume lithium slag waste comprehensive utilization technology and implementation method thereof

    CN111302708A

Cited By

  • Composite phase change energy storage material taking lithium slag-based geopolymer microspheres as carrier and preparation method of composite phase change energy storage material

    CN119331573A

  • Comprehensive recovery method of lithium slag

    CN120714773A

  • Yellow phosphorus slag-phosphogypsum-yellow phosphorus tailing mortar-based filling material as well as preparation method and application thereof

    CN120774685A

  • All-solid waste cementing material-based low-carbon low-heat high-crack-resistance mass concrete

    CN121517149A