High-strength and high-density fiber-modified wear-resistant and impact-resistant rubber concrete

By adding basalt fiber and epoxy resin to rubber concrete, the mechanical properties of rubber concrete are synergistically optimized, solving the problem of low compressive strength in the existing technology and significantly improving compression, impact resistance and wear resistance.

CN118754552APending Publication Date: 2024-10-11SICHUAN UNIV

Patent Information

Application Number
CN202410855569.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The compressive strength of existing rubber concrete is low, and fiber reinforcement research is mainly limited to a single fiber or a single polymer. There is no collaborative optimization research on basalt fiber and epoxy resin, resulting in its mechanical properties being inferior to traditional concrete.

Method used

Basalt fiber and epoxy resin are used as modifiers. By mixing basalt fiber and epoxy resin in different proportions, the mechanical properties of rubber concrete are improved and its compression resistance, impact resistance and wear resistance are enhanced.

Benefits of technology

The compression resistance, impact resistance and wear resistance of rubber concrete are significantly improved. When the BF content is 6kg/m3, the compression resistance and flexural resistance are the best, the abrasion resistance is increased by 256.87%, the wear rate is reduced by 59.3%, and the resistance to The impact strength is increased by 409.15%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754552A_ABST
    Figure CN118754552A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to high-strength and high-compactness fiber-modified wear-resistant impact-resistant rubber concrete. The wear-resistant impact-resistant modified rubber concrete is prepared from the following components in parts by weight: 354 parts of cement, 52 parts of silica fume, 87 parts of superfine cement, 87 parts of fly ash, 371.2 parts of sand, 1156 parts of stone, 128.57 parts of water, 8.7 parts of a water reducing agent, 30.21 parts of rubber powder, 92.8 parts of quartz sand, 6 parts of basalt fiber, 8 parts of epoxy resin and 4 parts of a curing agent. The high-strength and high-density fiber-modified wear-resistant and impact-resistant rubber concrete disclosed by the invention has relatively high mechanical properties, impact resistance and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a high-strength and high-density fiber-modified wear-resistant and impact-resistant rubber concrete. Background Art

[0002] Rubber concrete is a product that has been developed in recent years. Rubber concrete is made by grinding waste tires into rubber particles or rubber powder to replace part of the coarse aggregate, fine aggregate and cement in traditional concrete. As we all know, concrete is the most consumed building material in urban construction. Therefore, the large-scale use of rubber concrete can not only consume a large amount of waste tires and reduce the use of natural sand and gravel resources to achieve the purpose of protecting natural resources and reducing environmental pollution, but also has social and economic benefits. Studies have shown that adding rubber crumbs as a soft filler to concrete can improve the toughness, impact resistance, wear resistance, crack resistance and freeze-thaw cycle performance of concrete.

[0003] Although rubber concrete exhibits excellent energy absorption performance, previous studies have shown that the compressive strength of rubber concrete is reduced compared to traditional concrete. When the volume of rubber particles replaces 20% of natural sand, the compressive strength of concrete decreases by about 32%. This is because the bonding between rubber particles and cement matrix is ​​not as good as that of rigid aggregates, and the hydration products around rubber particles are limited, with obvious cracks and gaps, resulting in reduced strength of concrete. Therefore, improving the interfacial adhesion between rubber particles and cement matrix has become a key issue in promoting the use of rubber concrete.

[0004] Fiber-reinforced rubber concrete has attracted worldwide attention. The mechanical properties of concrete after fiber reinforcement are significantly improved. Basalt fiber reinforced concrete has been widely studied because of its high tensile strength, good cement bonding performance and excellent corrosion resistance. The bridging effect of basalt fiber can fill gaps or microcracks, which helps the strength, ductility and impact energy absorption of rubber concrete. These enhanced properties make rubber concrete better used in infrastructure projects such as dams, road pavements, and railway protection. At the same time, epoxy resin is a high molecular polymer that is often used to repair the interface of damaged concrete in dams due to its excellent bonding strength. Khashayar added epoxy resin to rubber concrete to make rubber polymer concrete. The results showed that the bonding performance was still good when the specimen failed, and the toughness was improved. Bulut filled unsaturated polyester resin into concrete and observed that the compressive strength of concrete increased with the increase of resin proportion, and the ideal resin content was 15%. Current research is limited to the reinforcement of single fiber or single polymer. Research on fiber-polymer composite optimization of rubber concrete bonding performance with basalt fiber reinforcement as the core has not been reported.

[0005] Compared with traditional concrete, rubber concrete has excellent deformation capacity, dynamic strength, high damping and high toughness, thus reducing the brittle failure exhibited by traditional concrete. However, due to the poor adhesion between rubber particles and cement mortar [11-13], and the rough surface of rubber, hydrophobicity and high Poisson's ratio, the mechanical properties of rubber concrete are inferior to those of ordinary concrete. Many studies have added fibers to rubber concrete to improve performance. Among them, the more common ones are steel fiber, carbon fiber, glass fiber, polypropylene fiber, etc. However, steel fiber and carbon fiber are expensive, glass fiber has poor durability, and polypropylene fiber is difficult to construct, resulting in that they cannot be used in large quantities. Basalt fiber has been a hot topic in recent years. It is not only low in cost, but also has better strength, toughness, ductility and crack resistance. Su et al. found that the addition of fibers reduced the degree of damage to rubber concrete, and Chen et al. found that basalt fibers reduced the brittleness of concrete, and the cracks produced in the specimens were small and uniform. At the same time, basalt fibers can reduce porosity and maximum pore size, and optimize the pore structure of concrete. In addition to fibers, some studies have used emulsified asphalt or colloidal nanosilica to modify rubber concrete. Epoxy resin is one of the most commonly used adhesives, used to provide better adhesion between concrete layers, thereby improving the bond strength. Nur et al. found that adding polymers such as epoxy resin to concrete can improve the adhesion and impermeability of concrete. Generally speaking, epoxy resin is used after mixing resin and hardener. The cured epoxy resin concrete has strong resistance to the atmosphere, moisture, chemical media, bacteria, etc., so it can be used in harsh environments. Adding epoxy resin to rubber concrete can be used as a repair material to compensate for the stiffness of concrete components. Yu et al. studied the effects of adding different fibers to polymer rubber concrete on the physical and mechanical properties, and explored the possibility of using this type of concrete as railway sleepers. Jin et al. studied the effects of curing agent type and curing temperature on the performance of epoxy resin concrete, and established a model for predicting early strength. However, the above-mentioned prior art is not in-depth enough in the study of the modified properties and mechanism of rubber concrete.

[0006] Based on this, it is urgent to understand the modification mechanism of BF and polymer, establish a prediction model for wear damage and impact damage, lay the foundation for the application of modified rubber concrete in hydraulic environment, and provide a BF modified rubber concrete. Summary of the invention

[0007] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-strength and high-density fiber-modified wear-resistant and impact-resistant rubber concrete, so as to at least achieve the effects of dense internal structure, good wear resistance and strong impact resistance.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] A wear-resistant and impact-resistant modified rubber concrete, wherein the raw materials include, by weight: 354 parts of cement, 52 parts of silica fume, 87 parts of ultrafine cement, 87 parts of fly ash, 371.2 parts of sand, 1156 parts of gravel, 128.57 parts of water, 8.7 parts of water reducing agent, 30.21 parts of rubber powder, 92.8 parts of quartz sand, 6 parts of basalt fiber, 8 parts of epoxy resin and 4 parts of curing agent.

[0010] Furthermore, the cement is PC42.5 Portland cement.

[0011] Furthermore, the rubber particles have a particle size of 1-3 mm.

[0012] Furthermore, the water reducer is a polycarboxylic acid high performance water reducer.

[0013] Further, the sand is the sand from the II zone mechanism;

[0014] And / or, the ultrafine cement is grade II ultrafine cement.

[0015] Furthermore, the particle size of the quartz sand is 300 μm.

[0016] Furthermore, the solid content of the waterborne epoxy resin is 47-53%, and the epoxy equivalent is 400-800 G / EQ.

[0017] Furthermore, the solid content of the curing agent is 42-46%, and the active hydrogen equivalent is 200-320.

[0018] Furthermore, the density of the basalt fiber is 2630 kg / m 3 , tensile strength is 3Gpa, and elastic modulus is 91GPa.

[0019] Furthermore, the stone is basalt crushed stone with a particle size of 4.75-16 mm and continuous grading.

[0020] It is worth noting that in this application:

[0021] The addition of epoxy resin polymer can improve fluidity and make the slump reach 66cm. BF can change the failure mode of the specimen and enhance the mechanical properties. The BF dosage is 6kg / m 3 , the compression and flexural properties are best when the solid-fat ratio is 4:8;

[0022] BF dosage is 6kg / m 3 The synergistic effect of epoxy resin polymer can improve the wear resistance of rubber concrete by up to 59.3%, but the polymer content should not exceed 8kg / m 3 ;

[0023] The solid-fat ratio is 4:8, and the BF dosage is 6kg / m3 When the BF content is 2kg / m 3 With 4kg / m 3 The strength of the specimens increased by 256.87% and 409.15%.

[0024] There is an obvious interface transition zone between rubber powder particles and cement matrix, which leads to a decrease in the strength of rubber concrete. BF can disperse the load and bridge the gap. Epoxy resin polymer can enhance cohesion and adsorb on the surface of rubber and BF in granular form, filling the pores, enhancing the adhesion between the two and the mortar, making the structure denser and playing a synergistic modification role. Figure 8 , showing the synergistic modification mechanism of BF and epoxy resin polymer. Figure 8 It can be seen that a part of the epoxy resin polymer will form particles and adsorb on the surface of BF and rubber powder particles to enhance the adhesion between the two and the mortar. At the same time, the granular polymer will fill the internal pores and cracks of the rubber concrete together with the calcium silicate to make the structure denser. This shows that adding epoxy resin polymer and BF to rubber concrete can reduce the negative effects of BF and rubber, and improve the mechanical properties and durability of rubber concrete.

[0025] The beneficial effects of the present invention are:

[0026] The present invention modifies rubber concrete (RC) by adding basalt fiber (BF), epoxy resin and curing agent mixture, and studies the mechanical properties, wear resistance and impact resistance of the modified rubber concrete. Among them, the epoxy resin polymer improves the fluidity of the rubber concrete, and the BF changes the failure mode of the rubber concrete and enhances the mechanical properties. Under all solid-to-fat ratios (curing agent and epoxy resin dosage ratios), the BF dosage is 6kg / m 3 When the rubber concrete has a high abrasion resistance, the wear rate is higher than that of the rubber concrete with a BF content of 2 kg / m 3 With 4kg / m 3 The average reduction of the specimens was 59.3% and 10.71%. The solid-to-fat ratio was 4:8 and the BF content was 6kg / m 3 Compared with BF dosage of 2kg / m 3 With 4kg / m 3 The impact strength of the specimens increased by 256.87% and 409.15%, showing significant improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a flow chart of the standard method for the test pouring process;

[0028] Figure 2This is a test diagram of the abrasion resistance of the modified rubber concrete in Example 1 after 12 hours of abrasion;

[0029] Figure 3 is a graph showing the wear rate of the modified rubber concrete in Example 2 when it is ground 40 times under a load of 200N;

[0030] Figure 4 is a graph showing the wear rate of the modified rubber concrete in Example 2 when it was ground 80 times under a load of 200N;

[0031] Figure 5 is a graph showing the wear rate of the modified rubber concrete in Example 2 when it was ground 120 times under a load of 200N;

[0032] Figure 6 The experimental device for the impact resistance test of Example 3;

[0033] Figure 7 This is a graph showing the impact strength test of the modified rubber concrete in Example 3;

[0034] Figure 8 This is the diagram of the synergistic modification mechanism of BF and epoxy resin polymer. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.

[0036] The sources or parameters of the raw materials used in the following examples are as follows:

[0037] Cement: density 3.13 g cm -3 ; Fineness 2.26%; Stability qualified; Setting time: initial setting 113min, final setting 237min; Compressive strength: 3d-24.8MPa, 28d-45.6MPa.

[0038] Basalt fiber: diameter 7-15μm, length 15mm, density 2630kg / m 3 , tensile strength 3GPa, elastic modulus 91Gpa.

[0039] Water-based epoxy resin: solid content 50±3%; PH2~7; specific gravity 1.01~1.08; viscosity <1000MPa·s, 25℃, epoxy equivalent 400~800G / EQ.

[0040] Mix design:

[0041] Prepare ingredients: Calculate the proportion of solid materials with different particle size distributions according to the most densely packed Dinger-Funk equation, and preliminarily design ordinary concrete based on strength grade C60, with a water-cement ratio of 0.55. Use rubber particles and quartz sand to replace the machine-made sand in equal volumes, with a replacement rate of 20%.

[0042] Then, different control groups were set up by changing the ratio of basalt fiber to epoxy resin. The basalt fiber dosage gradient was 2, 4 and 6 kg / m 3 The epoxy resin content is 4kg / m3 and 8kg / m3 respectively, and the curing agent content is 1kg / m 3 , 2kg / m 3 , 4kg / m 3 , where the solid fat mass ratio is determined to be 1:2 and 1:4 respectively. Table 1 lists all the mix ratios (unit: kg / m 3 ).

[0043] Table 1

[0044] serial number cement water gravel sand Fly ash Ultrafine cement Silica Fume Water reducing agent Quartz sand rubber Basalt fiber Epoxy resin Curing agent <![CDATA[BF2E4F1]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 2 4 1 <![CDATA[BF2E4F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 2 4 2 <![CDATA[BF2E8F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 2 8 2 <![CDATA[BF2E8F4]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 4 4 1 <![CDATA[BF4E4F1]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 4 4 2 <![CDATA[BF4E4F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 4 8 2 <![CDATA[BF4E8F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 4 8 4 <![CDATA[BF4E8F4]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 4 8 4 <![CDATA[BF6E4F1]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 6 4 1 <![CDATA[BF6E4F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 6 4 2 <![CDATA[BF6E8F2]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 6 8 2 <![CDATA[BF6E8F4]]> 354 128.6 1156 371.2 87 87 52 8.7 92.8 30.2 6 8 4

[0045] Specimen casting method:

[0046] The test pouring process is as follows Figure 1 As shown, after the rubber concrete specimens are prepared according to the steps, they are demoulded after drying and curing for 24 hours, and the performance test is carried out after water bath curing for 28 days.

[0047] Example 1 Abrasion resistance test

[0048] According to the above specimen casting method, the samples to be tested are cast into abrasion specimens of D×h=300mm×100mm and placed in a concrete abrasion resistance testing machine. According to the specification, the underwater steel ball method is used to flush for 12 hours, and the mass of the specimen is measured. The formula for abrasion resistance is: Where R a is the abrasion resistance, T is the scouring time, A is the scouring area of ​​the specimen, M T It is the quality difference of the specimen before and after flushing.

[0049] Test results such as Figure 2 The results show that: under all solid fat ratio conditions, the BF dosage is 2kg / m 3 With 4kg / m 3 The abrasion resistance of the specimens did not change significantly, only when the dosage reached 6kg / m 3The abrasion resistance of the specimens was significantly improved when the solid-fat ratio was 2:4, which was 108.41% higher than that of the specimens with other BF content. This shows that BF has a positive effect on abrasion resistance. Due to its bridging effect, the internal structure of the specimens is more compact, thus reducing mass loss. When the solid-fat ratio is 2:4, the specimen has the highest abrasion resistance of 30h / (kg / m 3 ), indicating that adding epoxy resin polymer and high-content BF to rubber concrete has the best effect on enhancing the abrasion resistance.

[0050] Example 2 Wear test

[0051] According to the above casting method, the sample is cast into a wear test specimen with a size of 150mm×150mm×40mm. The surface of the specimen is first polished smooth, and then ground 40, 80, and 120 times under a load of 200N on a cement mortar wear test machine and the mass is measured. The formula for wear resistance is: Where G c is the wear resistance, m1 is the mass of the specimen before grinding, and m2 is the mass of the specimen after grinding.

[0052] The wear rates of 40, 80 and 120 times are as follows: Figure 3 , Figure 4 and Figure 5 As shown, from Figure 3-5 It can be seen that the wear rate of the modified concrete is significantly improved. After 40, 80, and 120 times of wear, the average wear rate is 1.54 kg / m 2 3.68kg / m 2 , 4.7kg / m 2 Among them, BF has a positive effect on the wear rate. When the solid-fat ratio is 4:8 and the BF content is 2kg / m 3 When the specimen is worn for 80 and 120 times, there will be obvious mass loss, and the wear rate reaches 14.37kg / m 2 and 15.31kg / m 2 . BF dosage is 6kg / m 3 When the BF content is 2kg / m 3 With 4kg / m 3 The average reduction of the specimens is 59.3% and 10.71%, and the wear rate will not increase sharply. With the increase of epoxy resin polymer content, the wear rate curve of the specimen shows a trend of first decreasing and then increasing. After the polymer content is doubled, the wear rate of the specimen will increase by 11.42%, 16.78%, and 6.47% at different wear times. This shows that epoxy resin has an improvement effect on anti-wear performance, but the content should not exceed 8kg / m 3 .

[0053] Wear mechanism analysis: When friction occurs on the concrete surface, the process of stripping BF from the cement matrix consumes part of the load and disperses the wear force, reducing the amount of wear, thereby improving the wear resistance of the concrete. The uniform distribution of epoxy resin polymer can serve as a bridge transfer between different parts of the cement matrix, especially at cracks or internal pores, and the polymer film with high toughness integrates different parts in the mortar matrix, resulting in stress dispersion under high load conditions, thereby improving wear resistance. However, epoxy resin polymer will only have a modification effect when used in an appropriate amount. If the dosage is too small, the epoxy resin cannot form a continuous network, so it cannot provide a transfer effect and bonding effect. If the dosage is too high, it will carry more bubbles into the mortar system, and then form many pores, resulting in a decrease in the durability of the rubber concrete.

[0054] Experimental Example 3: Impact Test

[0055] According to the above casting method, the sample is cast into an impact test specimen with a size of 150mm×150mm×40mm. The experimental device is as follows: Figure 6 As shown. The test method is: fix the specimen directly below the iron ball, align the center of the iron ball with the center of the specimen, let the iron ball perform multiple free-fall movements, and record the number of falls when the first crack appears and the final destruction of the specimen. The formula for impact strength is: U = N × mgh; where U is the impact strength, N is the number of free falls of the iron ball, m is the mass of the iron ball, and h is the height.

[0056] Test results:

[0057] Concrete impact resistance test is an important means to evaluate the performance of concrete materials in harsh environments. Table 2 shows the average number of iron ball drops for the first crack (N1) and final destruction (N2) of the specimen. Figure 7 The impact failure mode of the specimen and the impact strength calculated according to the impact strength formula are given in:

[0058] Table 2

[0059] serial number <![CDATA[The first occurrence of cracks (N1)]]> <![CDATA[Final failure (N2)]]> <![CDATA[BF2E4F1]]> 3.7 4.3 <![CDATA[BF2E4F2]]> 10.7 11 <![CDATA[BF2E8F2]]> 4.7 5.7 <![CDATA[BF2E8F4]]> 3.7 4.7 <![CDATA[BF4E4F1]]> 5 5.7 <![CDATA[BF4E4F2]]> 4.3 5.3 <![CDATA[BF4E8F2]]> 2.7 3.3 <![CDATA[BF4E8F4]]> 3.3 4 <![CDATA[BF6E4F1]]> 2.3 3 <![CDATA[BF6E4F2]]> 8 8.7 <![CDATA[BF6E8F2]]> 8 9 <![CDATA[BF6E8F4]]> 16.7 17.3

[0060] From Table 2 and Figure 7 It can be seen that when the specimen was destroyed, many micro cracks appeared in the middle, and the specimen split into several pieces. As the BF content increased, the cracks produced when the specimen was destroyed gradually decreased. When the solid-to-fat ratio was 4:8 and the BF content was 6kg / m 3 When the BF content is 2kg / m 3 With 4kg / m 3 The strength of the specimens increased by 256.87% and 409.15%, respectively. This shows that high content of BF has a good effect on improving the impact strength of the specimens.

[0061] When the BF content is constant, the impact strength of the specimens with a solid-to-fat ratio of 2:4 (4:8) is 15.71 J higher than that of the specimens with a solid-to-fat ratio of 1:4 (2:8), and the specimen has a maximum strength of 73.98 J (BF6E8F4). Therefore, epoxy resin polymer should be added to rubber concrete at a solid-to-fat ratio of 4:8 with high content of BF, which can change the failure mode of rubber concrete and have better impact resistance.

[0062] Analysis of impact failure mechanism: In the early stage of impact failure, the lateral shear force and local compressive stress at the top of the specimen will cause matrix cracking and debonding between the BF and the matrix

[57] . However, BF can form a well-distributed fiber network. During the impact load, this fiber network effectively transfers energy to adjacent areas, thereby improving the overall energy dissipation capacity of the structure. Due to the presence of epoxy resin polymer, the connection between BF and cement matrix is ​​improved, and the bridging effect of BF will prevent the development of some cracks, resulting in delayed cracking and debonding. As the impact energy continues to increase, the BF breaks and the fibers at the bottom are pulled out due to bending stress. The specimen fails and splits into several pieces. When the content of BF and epoxy resin polymer is high, the failure mode of the specimen changes. The interlayer normal stress and shear stress will cause internal delamination of the specimen. Due to the micro-buckling of the fibers caused by the impact load, the specimen will not break completely during impact failure, but will produce fewer slender cracks in the upper part and absorb a large amount of impact energy.

[0063] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A wear-resistant and impact-resistant modified rubber concrete, characterized in that: By weight, the raw materials include: 354 parts of cement, 52 parts of silica fume, 87 parts of ultrafine cement, 87 parts of fly ash, 371.2 parts of sand, 1156 parts of gravel, 128.57 parts of water, 8.7 parts of water reducer, 30.21 parts of rubber powder, 92.8 parts of quartz sand, 6 parts of basalt fiber, 8 parts of epoxy resin, and 4 parts of curing agent.

2. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The cement is PC42.5 silicate cement.

3. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The particle size of the rubber particles is 1-3 mm.

4. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid high performance water reducing agent.

5. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The sand is the medium sand of Zone II mechanism; And / or, the ultrafine cement is grade II ultrafine cement.

6. The wear-resistant and impact-resistant concrete according to claim 5, characterized in that: The particle size of the quartz sand is 300 μm.

7. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The solid content of the waterborne epoxy resin is 47-53%, and the epoxy equivalent is 400-800 G / EQ.

8. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The solid content of the curing agent is 42-46%, and the active hydrogen equivalent is 200-320.

9. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The density of the basalt fiber is 2630kg / m 3 , tensile strength is 3Gpa, and elastic modulus is 91GPa.

10. The wear-resistant and impact-resistant concrete according to claim 1, characterized in that: The stone is basalt crushed stone with a particle size of 4.75-16mm and continuous grading.

Citation Information

Patent Citations

  • Modified rubber particle impact-resistant abrasion-resistant ultrahigh-toughness concrete and preparation method thereof

    CN110981327A

  • Wear-resistant impact-resistant high-strength rubber concrete and preparation method thereof

    CN116813268A

  • Impermeable concrete having polypropylene fiber and waste tire rubber particles added, and preparation method therefor

    WO2021227685A1

Cited By

  • Rubber concrete mix proportion design method and system

    CN121809291A