Road base mixture and preparation method thereof

CN118754553AInactive Publication Date: 2024-10-11MCC ENERGY SAVING & ENVIRONMENTAL PROTECTION +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410896555.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cost of obtaining raw materials for road infrastructure construction is high, and it is difficult to efficiently recycle and utilize construction waste, leading to resource supply bottlenecks and environmental pollution problems.

Method used

Waste autoclaved aerated concrete blocks and hot stuffy steel slag are used as raw materials. Through crushing, screening and mixing, a road base mixture is prepared, which is wet-mixed with cement and water to form aggregates and mixed under suitable conditions. Forming and curing.

Benefits of technology

It effectively improves the waste utilization rate, reduces the amount of natural sand and gravel, reduces quarrying and sand excavation in rivers, realizes resource recycling, reduces costs, and improves the compressive strength of the road base mixture.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a road base mixture and a preparation method thereof. The mixture is prepared from the following raw materials in parts by weight: 5-30 parts of concrete block recycled aggregate, 55-110 parts of pyrolytic steel slag recycled aggregate, 2-5 parts of cement and 3-21 parts of water. The preparation method comprises the following steps: preparing the concrete block recycled aggregate; preparing steel slag regenerated aggregate; and preparing a mixture: mixing the concrete block regenerated aggregate and the steel slag regenerated aggregate to obtain an aggregate, mixing and dispersing the aggregate and cement, and adding water for wet mixing to obtain the mixture. The problems that in the prior art, road infrastructure construction raw materials are high in obtaining cost, and construction waste is difficult to efficiently recycle and recycle can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of road engineering, and in particular to a road base mixture using waste autoclaved aerated concrete blocks and hot stuffy steel slag as raw materials and a preparation method thereof. Background Art

[0002] At present, large-scale road infrastructure construction in China requires a large amount of natural sand and gravel aggregates. With the country's regulation of mountain quarrying and river sand excavation, the price of sand and gravel has soared, and it is urgent to find alternative resources for natural sand and gravel. At the same time, with urban renewal projects, a large amount of construction waste will be generated. Among them, the annual amount of construction waste in large and medium-sized cities exceeds 2 billion tons. However, the effective utilization rate of construction waste is only 5%, far lower than the level of developed countries. The collection of sand and gravel, the generation of construction waste and the low recycling rate are all accompanied by endless development of resources and environmental problems.

[0003] It can be seen that in the process of rapid urban development, there is a dilemma that the cost of obtaining raw materials for road infrastructure construction is high, while construction waste is difficult to recycle efficiently. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present application provides a road base mixture using waste autoclaved aerated concrete blocks and hot-stifled steel slag as raw materials and a preparation method thereof, so as to solve the problems in the prior art that the raw materials for road infrastructure construction are expensive to obtain, while construction waste is difficult to efficiently recycle and utilize as resources.

[0005] In a first aspect of the present application, a road base mixture is provided, which is composed of the following raw materials in parts by weight: 5 to 30 parts of recycled aggregate of concrete blocks, 55 to 110 parts of recycled aggregate of hot-steamed steel slag, 2 to 5 parts of cement, and 3 to 21 parts of water.

[0006] Optionally, the concrete block recycled aggregate has a particle size of 0 to 5 mm (including 5 mm) and an apparent density of 2250 to 2350 kg / m 3 .

[0007] Optionally, the hot-stifled steel slag recycled aggregate is composed of the following steel slag particle size ratios by weight: 0-25 parts of steel slag with a particle size of 0-5mm (including 5mm), 25-35 parts of steel slag with a particle size of 5-10mm (including 10mm), 15-25 parts of steel slag with a particle size of 10-20mm (including 20mm), and 15-25 parts of steel slag with a particle size of 20-30mm (including 30mm).

[0008] Optionally, the apparent density of the hot smoldering slag is 3200-3700 kg / m 3 The water expansion rate of the hot-stifled steel slag is 0.1% to 1.9%.

[0009] Optionally, the cement is 42.5 grade ordinary Portland cement.

[0010] A second aspect of the present application provides a method for preparing a road base mixture, comprising the following steps:

[0011] Preparation of recycled aggregate of concrete blocks: waste autoclaved aerated concrete blocks from the demolition of building structure walls are selected, and the waste autoclaved aerated concrete blocks are crushed and sieved to obtain recycled aggregate particles of concrete blocks meeting the target particle size;

[0012] Preparation of steel slag recycled aggregate: Select steel slag treated by hot-pressing in a tank, crush and screen the hot-pressed steel slag to obtain steel slag recycled aggregate particles meeting the target particle size;

[0013] Preparation of mixture: The concrete block recycled aggregate and the steel slag recycled aggregate are mixed to obtain aggregate, the aggregate is mixed and dispersed with cement, and then water is added for wet mixing to obtain a mixture.

[0014] Optionally, obtaining recycled aggregate particles for concrete blocks meeting the target particle size includes selecting recycled aggregate particles for concrete blocks having a particle size of 0 to 5 mm (including 5 mm) and performing a pre-wetting treatment.

[0015] Optionally, the hot-stifled steel slag is crushed and screened to obtain steel slag recycled aggregate particles meeting the target particle size, including crushing the hot-stifled steel slag, screening and grading it into particles having the following particle size ranges: 0-5 mm (including 5 mm), 5-10 mm (including 10 mm), 10-20 mm (including 20 mm), and 20-30 mm (including 30 mm), and taking the required number of steel slag recycled aggregate particles according to the particle grading.

[0016] Optionally, the mixture is molded, shaped, and cured in sequence.

[0017] Optionally, the curing conditions are: temperature of 15-30° C. and humidity ≥95% RH.

[0018] The beneficial effects of this application are:

[0019] 1. This application uses waste autoclaved aerated concrete blocks and hot sultry steel slag as raw materials for road base mixtures. The waste autoclaved aerated concrete blocks that are difficult to use in construction waste and the steel slag that is the most difficult to use in the steel smelting industry are used in road base construction, which can not only solve the environmental pollution problems caused by the current large-scale storage of waste autoclaved aerated concrete blocks and steel slag, but also reduce mountain quarrying and river sand excavation, effectively alleviate the bottleneck of resource supply, realize the comprehensive utilization of waste autoclaved aerated concrete blocks and steel slag in the region, and promote the development of local circular economy and low-carbon economy;

[0020] 2. Compared with the prior art, the waste autoclaved aerated concrete blocks and hot-stifled steel slag road base mixture of the present application greatly increases the utilization of waste autoclaved aerated concrete blocks and steel slag, while realizing the coordinated disposal of multiple solid waste resources, providing a new disposal method for waste autoclaved aerated concrete blocks and steel slag producing areas; in addition, the method of the present application reduces the amount of cement used, replaces the expensive natural sand and gravel, and can save 5 to 18 yuan per square meter of water-stabilized material compared with the prior art.

[0021] 3. The method of this application not only realizes the low-cost production of base mixture, but also the unconfined compressive strength of the prepared waste autoclaved aerated concrete blocks and hot-stifled steel slag road base mixture can reach more than 10MPa after 7 days, so it has strong market competitiveness. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in conjunction with the specific embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0023] Concrete blocks are widely used in the walls of building structures in my country. Concrete blocks are widely used for their low density, good sound insulation and heat preservation effects, and convenient construction. However, they have low strength and high water absorption after demolition, making them difficult to use as high-strength concrete aggregates and can only be used as fine aggregates. On the other hand, the annual production of steel slag in large and medium-sized cities in my country exceeds 100 million tons, but the utilization rate of steel slag is only 30%. The volume stability of steel slag after tank-type pressure heat treatment is good, and it can be used as recycled coarse aggregate for base mixture without long-term storage and aging. In addition, steel slag also has hydraulic cementitious properties, and can be continuously hydrated and hardened in the later stage to improve the strength and anti-scouring properties of the road base.

[0024] Therefore, this application proposes to utilize concrete blocks in construction waste in conjunction with steelmaking slag to prepare road base mixture, which can effectively recycle construction waste and steel slag, realize resource utilization, and benefit the sustainable construction of urban infrastructure.

[0025] The embodiment of the present application provides a road base mixture, which is composed of the following raw materials in parts by weight: 5 to 30 parts of recycled aggregate of concrete blocks, 55 to 110 parts of recycled aggregate of hot-stifled steel slag, 2 to 5 parts of cement, and 3 to 21 parts of water.

[0026] In one embodiment of the present application, the added water is in an amount of 6-14% by mass of the total mass of the recycled aggregate of concrete blocks, the recycled aggregate of hot-stifled steel slag and the cement.

[0027] In one embodiment of the present application, the particle size distribution and apparent density of the recycled aggregate of the concrete block are measured. The particle size of the recycled aggregate of the concrete block is 0 to 5 mm (including 5 mm), and the apparent density is 2250 to 2350 kg / m 3 .

[0028] In one embodiment of the present application, the hot-stifled steel slag is steel slag that has been treated by a steel enterprise using a tank-type pressurized hot-stifling process; the hot-stifled steel slag is crushed, iron selected, and screened to obtain hot-stifled steel slag recycled aggregate; the particle size distribution, apparent density, and water expansion rate of the hot-stifled steel slag recycled aggregate are measured. The particle size distribution of the hot-stifled steel slag is 0-5mm, 5-10mm, 10-20mm, and 20-30mm, respectively, and the apparent density of the hot-stifled steel slag is 3200-3700kg / m 3 The water expansion rate of the hot-stifled steel slag is 0.1% to 1.9%.

[0029] Furthermore, the hot-stifled steel slag recycled aggregate is composed of the following steel slag particle size ratios by weight: 0-25 parts of steel slag with a particle size of 0-5mm (including 5mm), 25-35 parts of steel slag with a particle size of 5-10mm (including 10mm), 15-25 parts of steel slag with a particle size of 10-20mm (including 20mm), and 15-25 parts of steel slag with a particle size of 20-30mm (including 30mm).

[0030] In one embodiment of the present application, the road base mixture is composed of the following raw materials in parts by weight: 5 to 30 parts of recycled aggregate of concrete blocks with a particle size of 0 to 5 mm (including 5 mm), 0 to 25 parts of steel slag with a particle size of 0 to 5 mm (including 5 mm), 25 to 35 parts of steel slag with a particle size of 5 to 10 mm (including 10 mm), 15 to 25 parts of steel slag with a particle size of 10 to 20 mm (including 20 mm), 15 to 25 parts of steel slag with a particle size of 20 to 30 mm (including 30 mm), 2 to 5 parts of cement, and 3 to 21 parts of water.

[0031] In one embodiment of the present application, the apparent density of the hot smoldering slag is 3200-3700 kg / m 3 The water expansion rate of the hot-stifled steel slag is 0.1% to 1.9%.

[0032] In one embodiment of the present application, the cement is 42.5 grade ordinary Portland cement. Furthermore, the mass fraction of the cement is 2-5% of the total mass fraction of the waste autoclaved aerated concrete block recycled aggregate and the hot stuffy steel slag recycled aggregate.

[0033] It can be understood that age refers to the time that cement or mixture has experienced since the addition of water and mixing. 3d refers to 3 days since the addition of water and mixing. Under normal curing conditions, the strength of cement or mixture will continue to develop with the increase of age. The strength development is faster in the first 7 to 14 days, and then gradually slows down. The design strength is reached in 28 days, and its strength grade is determined based on the 28-day compressive strength. The strength is still developing after 28 days, and its growth process can continue for decades. Under standard curing conditions, the development of cement or mixture strength is roughly proportional to the common logarithm of its age (age is not less than 3d).

[0034] In the present application, the standard compressive strength and flexural strength of the cement at 3 days of age are 27.4 and 5.5 MPa, respectively, and the standard compressive strength and flexural strength at 28 days of age are 53.6 and 8.7 MPa, respectively.

[0035] The present invention provides a method for preparing a road base mixture, comprising the following steps:

[0036] Preparation of recycled aggregate of concrete blocks: waste autoclaved aerated concrete blocks from the demolition of building structure walls are selected, and the waste autoclaved aerated concrete blocks are crushed and sieved to obtain recycled aggregate particles of concrete blocks meeting the target particle size;

[0037] Preparation of steel slag recycled aggregate: Select steel slag treated by hot-pressing in a tank, crush and screen the hot-pressed steel slag to obtain steel slag recycled aggregate particles meeting the target particle size;

[0038] Preparation of mixture: The concrete block recycled aggregate and the steel slag recycled aggregate are mixed to obtain aggregate, the aggregate is mixed and dispersed with cement, and then water is added for wet mixing to obtain a mixture.

[0039] In one embodiment of the present application, the obtaining of recycled aggregate particles for concrete blocks that meet the target particle size includes selecting recycled aggregate particles for concrete blocks with a particle size of 0 to 5 mm (including 5 mm) and pre-wetting them. Due to the low water-cement ratio of concrete materials, severe self-shrinkage often occurs during the preparation process. In the past, expansion agents were added to concrete to solve the problem of concrete shrinkage. The present application can effectively reduce the degree of self-shrinkage by pre-wetting the recycled aggregate particles for concrete blocks. In one embodiment of the present application, the recycled aggregate particles for concrete blocks are soaked or covered with water to achieve humidity balance, and the pre-wetting time of the pre-wetting treatment is 1 to 3 hours.

[0040] In one embodiment of the present application, the hot stuffy steel slag is crushed and screened to obtain steel slag recycled aggregate particles that meet the target particle size, including crushing the hot stuffy steel slag and screening and grading it into particles in the following particle size ranges according to the particle size: 0-5mm (including 5mm), 5-10mm (including 10mm), 10-20mm (including 20mm), 20-30mm (including 30mm), and taking the required number of steel slag recycled aggregate particles according to the particle size distribution. Of course, in addition to the particle sizes listed in this embodiment, there may be other ranges of steel slag particle sizes, which can be further recycled to avoid waste.

[0041] Furthermore, after the hot stuffy slag is crushed, an iron selection operation is further performed. The slag is the molten slag discharged during the steelmaking process, which is mainly composed of oxides generated after the elements in the metal charge are oxidized, corroded furnace lining materials and furnace filling materials, impurities brought into the metal charge, and slag-making materials specially added for the needs of smelting different types of steel, resulting in an iron content of 3% to 4% in the slag. The iron content of the slag discharged by my country's steel industry reaches more than 15 million tons per year. The present application further effectively removes the iron in the slag through the slag iron selection process, which not only reduces the difficulty of slag crushing and grinding, improves the quality of slag ore powder products, but also can reduce the waste of a large amount of iron resources. The slag iron selection process can separate iron particles and iron powder. The iron content in the treated slag tailings is usually less than 1%, and the iron recovery rate in the slag is high. The hot stuffy slag is crushed and screened after iron selection.

[0042] In one embodiment of the present application, after the mixture is prepared, the mixture is sequentially molded, shaped, a road base pavement is constructed, and then maintained.

[0043] The curing conditions are as follows: temperature of 15-30° C. and humidity ≥95% RH.

[0044] Specifically, during the mold installation process, keep the inner wall of the mold clean. A thin layer of release agent such as mineral oil can be evenly applied on the inner wall, and the release agent should be evenly distributed without obvious deposition.

[0045] Determine the appropriate molding method based on factors such as the consistency of the mixture to ensure that the concrete is fully compacted and avoid stratification and segregation. For example, a vibrating table or a manual vibrator can be used for compaction. After that, a film or a weight plate can be pressed on the surface to facilitate molding. After molding, demoulding is carried out, and the road base pavement is constructed according to the construction plan and maintained.

[0046] It should be noted that the raw material component contents in the present application include endpoint values, such as 2 to 5 parts of cement, which means: 2 parts ≤ parts by weight of fly ash ≤ 5 parts by weight.

[0047] The present application also provides a method for preparing a road base mixture specimen, which is implemented by the following steps:

[0048] 1) Use waste autoclaved aerated concrete blocks from the demolition of building structure walls and steel slag that has been treated with hot and cold pressure in a tank;

[0049] 2) The waste autoclaved aerated concrete blocks are crushed and screened to obtain 0-5 mm recycled fine aggregates, and the hot suffocated steel slag is crushed, magnetically separated and iron removed, and screened to obtain 0-5 mm, 5-10 mm, 10-20 mm, and 20-30 mm recycled aggregates;

[0050] 3) Pre-wetting the waste autoclaved aerated concrete blocks, and then mixing them with hot and stuffy steel slag in proportion to form aggregate;

[0051] 4) adding cement to aggregates and mixing them to obtain waste autoclaved aerated concrete blocks and hot-stifled steel slag base mixture;

[0052] 5) The waste autoclaved aerated concrete blocks and the hot-stifled steel slag base mixture are loaded into a mold, and a small pressure machine is used for vibration compaction. After compaction, the mixture is placed in a curing box for curing for 7 days before demoulding.

[0053] Example 1

[0054] The waste autoclaved aerated concrete blocks and hot-stifled steel slag base mixture in this embodiment are composed of the following ingredients in parts by weight: 5 parts of recycled aggregate for concrete blocks with a particle size of 0-5mm (including 5mm), 25 parts of steel slag with a particle size of 0-5mm (including 5mm), 30 parts of steel slag with a particle size of 5-10mm (including 10mm), 20 parts of steel slag with a particle size of 10-20mm (including 20mm), 20 parts of steel slag with a particle size of 20-30mm (including 30mm), 4 parts of cement, and 8 parts of water.

[0055] The raw materials were weighed according to the above proportions. The waste autoclaved aerated concrete block recycled aggregate was pre-wetted and then mixed with steel slag aggregate, and then cement and water were added to make the waste autoclaved aerated concrete block and hot-stifled steel slag base mixture. The mixture was loaded into the mold and compacted by a small pressure mechanical vibration mode. After compaction, it was placed in a curing box and cured for 7 days before demoulding. A 7-day-old road base mixture specimen was obtained.

[0056] Example 2

[0057] The waste autoclaved aerated concrete blocks and hot-stifled steel slag base mixture in this embodiment are composed of the following ingredients in parts by weight: 10 parts of recycled aggregate for concrete blocks with a particle size of 0-5mm (including 5mm), 20 parts of steel slag with a particle size of 0-5mm (including 5mm), 30 parts of steel slag with a particle size of 5-10mm (including 10mm), 20 parts of steel slag with a particle size of 10-20mm (including 20mm), 20 parts of steel slag with a particle size of 20-30mm (including 30mm), 4 parts of cement, and 9 parts of water.

[0058] The raw materials were weighed according to the above proportions. The waste autoclaved aerated concrete block recycled aggregate was pre-wetted and then mixed with steel slag aggregate, and then cement and water were added to make the waste autoclaved aerated concrete block and hot-stifled steel slag base mixture. The mixture was loaded into the mold and compacted by a small pressure mechanical vibration mode. After compaction, it was placed in a curing box and cured for 7 days before demoulding. A 7-day-old road base mixture specimen was obtained.

[0059] Example 3

[0060] The waste autoclaved aerated concrete blocks and hot-stifled steel slag base mixture in this embodiment are composed of the following ingredients in parts by weight: 20 parts of recycled aggregate for concrete blocks with a particle size of 0-5mm (including 5mm), 10 parts of steel slag with a particle size of 0-5mm (including 5mm), 30 parts of steel slag with a particle size of 5-10mm (including 10mm), 20 parts of steel slag with a particle size of 10-20mm (including 20mm), 20 parts of steel slag with a particle size of 20-30mm (including 30mm), 4 parts of cement, and 10 parts of water.

[0061] The raw materials were weighed according to the above proportions. The waste autoclaved aerated concrete block recycled aggregate was pre-wetted and then mixed with steel slag aggregate, and then cement and water were added to make the waste autoclaved aerated concrete block and hot-stifled steel slag base mixture. The mixture was loaded into the mold and compacted by a small pressure mechanical vibration mode. After compaction, it was placed in a curing box and cured for 7 days before demoulding. A 7-day-old road base mixture specimen was obtained.

[0062] Example 4

[0063] The waste autoclaved aerated concrete blocks and hot-stifled steel slag base mixture in this embodiment are composed of the following ingredients in parts by weight: 30 parts of recycled aggregate for concrete blocks with a particle size of 0-5mm (including 5mm), 0 parts of steel slag with a particle size of 0-5mm (including 5mm), 30 parts of steel slag with a particle size of 5-10mm (including 10mm), 20 parts of steel slag with a particle size of 10-20mm (including 20mm), 20 parts of steel slag with a particle size of 20-30mm (including 30mm), 4 parts of cement, and 12 parts of water.

[0064] The raw materials were weighed according to the above proportions. The waste autoclaved aerated concrete block recycled aggregate was pre-wetted and then mixed with steel slag aggregate, and then cement and water were added to make the waste autoclaved aerated concrete block and hot-stifled steel slag base mixture. The mixture was loaded into the mold and compacted by a small pressure mechanical vibration mode. After compaction, it was placed in a curing box and cured for 7 days before demoulding. A 7-day-old road base mixture specimen was obtained.

[0065] Comparative Example

[0066] In this comparative example, a base mixture was prepared, and the mixture consisted of the following ingredients in parts by weight: 30 parts of natural river sand with a particle size of 0-5mm (including 5mm), 0 parts of steel slag with a particle size of 0-5mm (including 5mm), 30 parts of natural gravel with a particle size of 5-10mm (including 10mm), 20 parts of natural gravel with a particle size of 10-20mm (including 20mm), 20 parts of natural gravel with a particle size of 20-30mm (including 30mm), 4 parts of cement, and 12 parts of water.

[0067] Weigh the raw materials according to the above proportions, mix natural river sand and natural crushed stone, add cement and water to mix, and make the base mixture. Put it into the mold and use a small pressure mechanical vibration compaction mode. After compaction and molding, put it into the curing box and curing for 7 days before demoulding. Obtain the 7d-old road base mixture specimen.

[0068] The 7-day-old road base mixture specimens containing waste autoclaved aerated concrete blocks and hot-stifled steel slag aggregate prepared in Examples 1 to 4, as well as the 7-day-old base mixture specimens prepared in the comparative example, were subjected to unconfined compressive strength tests one by one. The test results are shown in Table 1 for the compressive strength test results.

[0069] Table 1 Compressive strength test results

[0070] Serial number Specimen size Compressive strength(MPa) Example 1 Ф100mm*100mm 16.21 Example 2 Ф100mm*100mm 14.08 Example 3 Ф100mm*100mm 13.74 Example 4 Ф100mm*100mm 12.63 Comparative Example Ф100mm*100mm 10.18

[0071] As can be seen from Table 1, the 7-day unconfined compressive strength of the road base mixture specimens prepared in Examples 1 to 4 can reach more than 10 MPa, which is better than the unconfined compressive strength of the base mixture prepared with natural aggregates.

[0072] In addition, in Examples 1 to 4, the content of recycled aggregate in concrete blocks is increasing, the content of steel slag aggregate is decreasing, and the compressive strength of the test pieces is decreasing, which shows that Example 1 is a better example in this application. Examples 1 to 4 can all meet the strength requirements of road base components, and adding steel slag aggregate to the road base mixture can effectively improve the compressive strength.

[0073] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A road base mixture, characterized in that: The invention is composed of the following raw materials in parts by weight: 5 to 30 parts of recycled aggregate of concrete blocks, 55 to 110 parts of recycled aggregate of hot-stifled steel slag, 2 to 5 parts of cement and 3 to 21 parts of water.

2. A road base mixture as claimed in claim 1, characterized in that: The concrete block recycled aggregate particle size is 0-5mm (including 5mm), and the apparent density is 2250-2350kg / m 3 .

3. A road base mixture as claimed in claim 1, characterized in that: The hot-stifled steel slag recycled aggregate is composed of the following steel slag particle size ratios by weight: 0-25 parts of steel slag with a particle size of 0-5 mm (including 5 mm), 25-35 parts of steel slag with a particle size of 5-10 mm (including 10 mm), 15-25 parts of steel slag with a particle size of 10-20 mm (including 20 mm), and 15-25 parts of steel slag with a particle size of 20-30 mm (including 30 mm).

4. A road base mixture as claimed in claim 1, characterized in that: The apparent density of the hot smoldering slag is 3200-3700 kg / m 3 The water expansion rate of the hot-stifled steel slag is 0.1% to 1.9%.

5. A road base mixture as claimed in claim 1, characterized in that: The cement is 42.5 grade ordinary Portland cement.

6. A method for preparing a road base mixture, characterized in that: The following steps are involved: Preparation of recycled aggregate of concrete blocks: waste autoclaved aerated concrete blocks from the demolition of building structure walls are selected, and the waste autoclaved aerated concrete blocks are crushed and sieved to obtain recycled aggregate particles of concrete blocks meeting the target particle size; Preparation of steel slag recycled aggregate: Select steel slag treated by hot-pressing in a tank, crush and screen the hot-pressed steel slag to obtain steel slag recycled aggregate particles meeting the target particle size; Preparation of mixture: The concrete block recycled aggregate and the steel slag recycled aggregate are mixed to obtain aggregate, the aggregate is mixed and dispersed with cement, and then water is added for wet mixing to obtain a mixture.

7. A method for preparing a road base mixture according to claim 6, characterized in that: The method of obtaining recycled aggregate particles of concrete blocks meeting the target particle size includes selecting recycled aggregate particles of concrete blocks having a particle size of 0 to 5 mm (including 5 mm) and performing a pre-wetting treatment.

8. A method for preparing a road base mixture according to claim 6, characterized in that: The method of crushing and screening the hot-stifled steel slag to obtain steel slag recycled aggregate particles meeting the target particle size includes crushing the hot-stifled steel slag, screening and grading the particles into particles having the following particle size ranges: 0-5 mm (including 5 mm), 5-10 mm (including 10 mm), 10-20 mm (including 20 mm), and 20-30 mm (including 30 mm), and taking the required number of steel slag recycled aggregate particles according to the particle grading.

9. A method for preparing a road base mixture according to claim 6, characterized in that: The mixed material is molded, shaped and cured in sequence.

10. A method for preparing a road base mixture according to claim 6, characterized in that: The curing conditions are as follows: temperature of 15-30° C. and humidity ≥95% RH.