NPO energy storage dielectric ceramic material, preparation method and application thereof

By adding MnO and MnO2 to NPO ceramic materials, manganese-doped NPO energy storage dielectric ceramic materials are prepared using solid-state reaction methods, which solves the problem of insufficient dielectric properties of ceramic materials and achieves high dielectric constant and low dielectric properties. Ceramic material with electrical loss and high voltage resistance, suitable for applications such as high-frequency circuits and oscillators.

CN118754643APending Publication Date: 2024-10-11BAOJI UNIV OF ARTS & SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410857050.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing NPO ceramic materials have performance defects such as low room temperature dielectric constant, low voltage strength, and large dielectric loss, making it difficult to meet the requirements of applications such as high-frequency circuits and oscillators.

Method used

The solid-state reaction method is used to prepare manganese-doped NPO energy storage dielectric ceramic materials. MnO and MnO2 are added as dopants into the ceramic materials to adjust the electrical properties of the materials. The specific steps include ball milling, drying, pre-sintering and sintering. Forms ceramic flakes with excellent dielectric properties.

Benefits of technology

The room temperature dielectric constant of the ceramic material is increased to 120-125, the dielectric loss is reduced to 0.0003-0.0010, the compressive strength is improved, and the process is simple and low-cost, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754643A_ABST
    Figure CN118754643A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of energy storage ceramic materials, and particularly relates to an NPO energy storage dielectric ceramic material and a preparation method and application thereof. According to the preparation method, manganese-doped NPO powder is prepared by adopting a solid-phase reaction method, and the manganese-doped NPO energy storage dielectric ceramic material is prepared by sintering; the thickness of the prepared manganese-doped NPO energy storage dielectric ceramic sheet material is within the range of 1.30-1.60 mm, the grain size distribution is uniform, and the compactness degree is good; the prepared fine-grain energy-storage ceramic capacitor dielectric material has the advantages that the room-temperature dielectric constant reaches 120 or above, and the compression strength is higher; the dielectric loss of the fine-grain energy-storage ceramic capacitor dielectric material prepared by the invention is only 0.0004, so that the dielectric loss is small; the prepared ceramic is uniform in particle size, high in reliability and suitable for being used for producing a ceramic energy storage capacitor with a large-capacity and ultrathin dielectric layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy storage ceramic materials, and in particular relates to a NPO energy storage dielectric ceramic material, a preparation method and application thereof. Background Art

[0002] At present, there are two methods for preparing ceramic materials: solid phase method and wet chemical method. The solid phase method is a method of obtaining powder from solid raw materials through chemical reaction. Although the powder prepared by the solid phase method has some disadvantages, it may cause the dielectric properties of the final capacitor to be unstable. However, the solid phase method has the advantages of high yield, low cost, simple process, environmental stability, large-scale production, low environmental pollution, and does not involve complicated washing process compared with the wet chemical method, so it is used by most domestic manufacturers.

[0003] NPO type MLCC capacitors have temperature compensation characteristics, which not only meet the requirements of high capacitance, but also have excellent electrical properties. As a type of capacitor with the most stable capacitance and dielectric loss, they are used in oscillators, resonators and high-frequency circuits. 2 As the main component, its capacitance basically does not change with temperature, time, voltage, etc. In an environment with large temperature changes, its capacitance value can also remain relatively stable.

[0004] However, a large number of studies have shown that a single type of ceramic material will have some performance defects (Gong Xue, Zhao Huilin, Liu Wei. A review of research on the modification of lead-free ferroelectric ceramic materials by doping [J]. Juye, 2022, 179 (12): 64-66). In order to make ceramic materials obtain more superior performance, researchers have modified the materials through reasonable approaches. The commonly used methods currently studied are mainly ion doping, coating modification, and composite ceramic modification. Among them, ion doping and composite ceramic modification are considered to be two effective methods. A large number of studies have shown that non-rare earth element Mn is an effective dopant to improve the electrical properties of ceramics. Moreover, Mn has many attractive advantages, such as good conductivity and excellent charge storage capacity; the doping of Mn ions effectively increases the number of oxygen vacancies, changes the local electronic structure, promotes charge transfer and ion migration of the electrode, and minimizes Ti 4+ The reduction in the sintering process reduces the leakage current of the material in the high voltage electric field and improves the electrical properties. According to the valence state of Mn ions, different valence ions have different effects on the properties of ceramics, such as Mn 4+ As a donor dopant, MnO can increase the piezoelectric constant of the material and reduce the DC conductivity. 2 When used as a sintering aid, it can also enhance the densification of ceramics; Mn 2+ As an acceptor dopant, it will enter the B site and reduce the electric field leakage current.2 and MnO, added into NPO energy storage dielectric ceramic materials by solid phase method, can solve the performance defects of existing NPO ceramic materials such as low room temperature dielectric constant, low compressive strength and large dielectric loss.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and provide a NPO energy storage dielectric ceramic material, a preparation method and application thereof.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] On the one hand, the present invention provides a NPO energy storage dielectric ceramic material, wherein the proportions of the components are as follows, based on mass percentage: the main component is 15-30% BaTiO 3 20-40% Sm 2 O 3 , 15-30% Bi 2 O 3 30-50% TiO 2 , 0.16-0.53% manganese oxide, additive 0.1-1.0% V 2 O 5 , 0.1-0.5% Sb 2 O 3 , 0.1-0.5% SiO 2 , 0.1-0.5% Al 2 O 3 , 1.5-2.0% SrO; wherein the manganese oxide is MnO and MnO 2 .

[0009] Specifically, the room temperature dielectric constant of the NPO energy storage dielectric ceramic material is 120-125.

[0010] Specifically, the room temperature dielectric loss of the NPO energy storage dielectric ceramic material is 0.0003-0.0010.

[0011] On the other hand, the present invention provides a method for preparing an NPO energy storage dielectric ceramic material, specifically: firstly weighing the required raw materials according to the mass fraction ratio, then preparing manganese-doped NPO powder by a solid phase reaction method, and finally sintering to prepare the NPO energy storage dielectric ceramic material.

[0012] Specifically, the preparation steps are as follows:

[0013] Step 1: Calculate the mass of various raw materials required according to the mass fraction ratio and weigh them, the raw materials include but are not limited to (CH 3 COO 2 Ba、Sm 2 O 3 、Bi 2 O 3 、TiO 2 , Additive V 2 O 5 , Sb 2 O 3 、SiO 2 , (CH 3 COO 3 Al, (CH 3 COO 2 At least one of Sr, (CH 3 COO 2 Mn;

[0014] Then, the weighed raw materials were added into the ball mill, and ethanol, pure water, powder, and zirconium oxide beads were added into the ball mill in a mass ratio of 1:2:3:9;

[0015] Step 2: After grinding in the ball mill for 0.5-1h, reduce the speed and continue ball milling for 8-12h;

[0016] Step 3: Place the ground slurry in an oven at 60-80°C and dry until completely dry;

[0017] Step 4, transfer the dried powder to a clean and dry crucible, set the heating rate to 2℃ / min from room temperature to 400-600℃, keep warm for 30-60min, then heat to 800-1000℃ at 4℃ / min, keep warm for 0.5-1h, then heat to 900-1100℃ at 4℃ / min, keep warm for 1-2h, and then wait for the powder temperature to drop to room temperature before taking it out for use;

[0018] Step 5: Pour the pre-burned powder into an agate mortar, add 3 drops of polyvinyl alcohol (PVA) to the agate mortar according to the ratio of 1g of powder to 3 drops of PVA, and grind manually. Grind in a clockwise direction until there are no large particles and the powder is fine and smooth, then stop grinding.

[0019] Step 6, weigh 0.5g of the ground powder, pour it into the corresponding mold, press it into a thin sheet with a diameter of 10mm and uniform texture, and then put it into a marked ziplock bag for standby use; the thickness of the thin sheet is 1.30-1.60mm;

[0020] Step 7. Spread a thick layer of zirconium oxide on the zirconium plate to prevent deformation of the ceramic during high-temperature sintering. The heating rate of the sintering process is set to 2°C / min from room temperature to 400-600°C, keep warm for 30-60min, heat up to 800-1000°C at 4°C / min, keep warm for 0.5-1h, then heat up to 1200-1260°C at 4°C / min, keep warm for 0.5-2h, and then cool to room temperature to obtain NPO energy storage dielectric ceramic material.

[0021] On the other hand, the present invention provides an application of the NPO energy storage dielectric ceramic material prepared by the above preparation method, and the NPO energy storage dielectric ceramic material is used in, including but not limited to, preparing oscillators, resonators, and high-frequency circuits.

[0022] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0023] The NPO energy storage dielectric ceramic material of the present invention has a room temperature dielectric constant of more than 120 and a high compressive strength; the dielectric loss is only 0.0004, the dielectric loss is small, and the reliability is strong; the powder prepared by the preparation method has a uniform particle size, and the preparation method also has the characteristics of simple process and low cost, and is suitable for large-scale promotion;

[0024] Furthermore, the ceramic material prepared by the present invention has uniform particle size and high reliability, and is suitable for producing ceramic energy storage capacitors with large capacity and ultra-thin dielectric layers;

[0025] Furthermore, the manganese-doped NPO energy storage dielectric ceramic sheet prepared by the present invention has a thickness in the range of 1.30 to 1.60 mm, a uniform grain size distribution, and a good degree of compactness. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0028] Figure 1 XRD diagrams of powder samples #1-1, #1-2, #1-3, #1-4, and #1-5 in Example 1;

[0029] Figure 2 The SEM images of the powder samples #1-1, #1-2, #1-3, #1-4 and #1-5 in Example 1 are shown;

[0030] Figure 3 XRD patterns of ceramic samples #1-6, #1-7, #1-8, #1-9, and #1-10 in Example 1;

[0031] Figure 4 The SEM images of the ceramic samples #1-6, #1-7, #1-8, #1-9 and #1-10 in Example 1;

[0032] Figure 5 This is the EDS graph of the ceramic sample in Example 1 when the manganese doping amount is 0.53wt%;

[0033] Figure 6 The characteristic curve diagram of the dielectric constant of the ceramic samples #1-6, #1-7, #1-8, #1-9 and #1-10 in Example 1 as a function of temperature;

[0034] Figure 7 XRD diagrams of ceramic samples #2-1, #2-2, and #2-3 in Example 2;

[0035] Figure 8 The SEM images of the ceramic samples #2-1, #2-2 and #2-3 in Example 2;

[0036] Fig. 9 This is a characteristic curve diagram of the dielectric constant of ceramic samples #2-1, #2-2, and #2-3 in Example 2 changing with temperature. DETAILED DESCRIPTION

[0037] Exemplary embodiments are described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims; manganese doping in the text refers to manganese oxide MnO and MnO 2 Doped into existing NPO energy storage dielectric ceramic materials to improve performance.

[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0039] The present invention provides a method for preparing a NPO energy storage dielectric ceramic material, and the specific steps are as follows:

[0040] Step 1: Calculate the mass of various raw materials required according to the mass fraction ratio and weigh them, the raw materials include but are not limited to (CH 3 COO 2Ba、Sm 2 O 3 、Bi 2 O 3 、TiO 2 , Additive V 2 O 5 , Sb 2 O 3 、SiO 2 , (CH 3 COO 3 Al, (CH 3 COO 2 At least one of Sr, (CH 3 COO 2 Mn;

[0041] Then, the weighed raw materials were added into the ball mill, and ethanol, pure water, powder, and zirconium oxide beads were added into the ball mill in a mass ratio of 1:2:3:9;

[0042] Step 2, after grinding in a ball mill for 0.5-1h, reduce the speed and ball mill for 8-12h;

[0043] Step 3: Place the ground slurry in an oven at 60-80°C and dry until completely dry;

[0044] Step 4, transfer the dried powder to a clean and dry crucible, set the heating rate to 2℃ / min from room temperature to 400-600℃, keep warm for 30-60min, then heat to 800-1000℃ at 4℃ / min, keep warm for 0.5-1h, then heat to 900-1100℃ at 4℃ / min, keep warm for 1-2h, and then wait for the powder temperature to drop to room temperature before taking it out for use;

[0045] Step 5: Pour the pre-burned powder into an agate mortar, add 3 drops of polyvinyl alcohol (PVA) to the agate mortar according to the ratio of 1g of powder to 3 drops of PVA, and grind manually. Grind in a clockwise direction until there are no large particles and the powder is fine and smooth, then stop grinding.

[0046] Step 6, weigh 0.5g of the ground powder, pour it into the corresponding mold, press it into a thin sheet with a diameter of 10mm and uniform texture, and then put it into a marked ziplock bag for standby use; the thickness of the thin sheet is 1.30-1.60mm;

[0047] Step 7: Spread a thick layer of zirconium oxide on the zirconium plate to prevent deformation of the thin sheet during high-temperature sintering. During the sintering process, the temperature is increased from room temperature to 400-600°C at a rate of 2°C / min, kept warm for 30-60min, then increased to 800-1000°C at a rate of 4°C / min, kept warm for 0.5-1h, then increased to 1200-1260°C at a rate of 4°C / min, kept warm for 0.5-2h, and then cooled to room temperature to obtain a manganese-doped NPO energy storage dielectric ceramic material.

[0048] In order to further verify the characteristics of manganese-doped NPO powder and its ceramic material, the present invention also provides the following examples:

[0049] Example 1

[0050] Manganese-doped NPO powders with different contents and ceramic materials thereof were prepared, wherein the mass fraction of manganese doping was 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%. The corresponding powders of different manganese-doped NPO were recorded as #1-1, #1-2, #1-3, #1-4, and #1-5, and the serial numbers of the ceramic samples were #1-6, #1-7, #1-8, #1-9, and #1-10, respectively. The embodiment was used to prepare NPO powders with different mass fractions of manganese doped and ceramic materials thereof.

[0051] The specific steps of the material are as follows:

[0052] (1) Calculate the mass of various raw materials required according to the molecular formula and mass fraction, including but not limited to (CH 3 COO 2 Ba、Sm 2 O 3 、Bi 2 O 3 、TiO 2 , Additive V 2 O 5 , Sb 2 O 3 、SiO 2 , (CH 3 COO 3 Al, (CH 3 COO 2 At least one of Sr, (CH 3 COO 2 Mn; accurately weigh with an electronic analytical balance, add the weighed raw materials into a clean ball mill, add ethanol, pure water and clean zirconia beads into the ball mill according to the mass ratio of ethanol: pure water: powder = 1:2:3, zirconia beads: powder = 3:1;

[0053] (2) Fix the ball mill jar to the ball mill and tighten the nut, adjust the speed to 400 r / min, and adjust the speed to 300 r / min after 30 minutes, and ball mill at a speed of 300 r / min for 10 hours;

[0054] (3) Dry the ground slurry in an oven at 60°C until completely dry;

[0055] (4) The dried powder is transferred to a clean and dry crucible for pre-sintering. The heating rate is set to 2°C / min from room temperature to 500°C, kept at this temperature for 30 min, then raised to 900°C at 4°C / min, kept at this temperature for 1 h, then raised to 1000°C at 4°C / min, kept at this temperature for 2 h, and then the powder temperature is taken out after it drops to room temperature for use;

[0056] (5) Pour the pre-burned powder into an agate mortar, add 3 drops of polyvinyl alcohol (PVA) at a ratio of 1 gram of powder, and grind in a clockwise direction until no large particles are left and the powder is fine and smooth;

[0057] (6) Weigh 0.5 g of the powder into a mold and press it into a uniform sheet with a diameter of 10 mm;

[0058] (7) A thick layer of zirconium oxide was spread on the zirconium plate to prevent deformation of the ceramic during high-temperature sintering. The heating rate during the sintering process was set to increase from room temperature to 500°C at 2°C / min, keep warm for 30 min, increase to 900°C at 4°C / min, keep warm for 1 h, and then increase to 1230°C at 4°C / min. After keeping warm for 2 h, the ceramic samples were cooled to room temperature to obtain five ceramic samples.

[0059] in, Figure 1 These are the XRD patterns of powder samples #1-1, #1-2, #1-3, #1-4, and #1-5 (XRD is a technique that uses the diffraction effect of X-rays in crystalline materials to analyze the structure of materials, where the horizontal axis in the figure is the 2θ angle and the vertical axis is the relative intensity. In the figure, #1-1, #1-2, #1-3, #1-4, and #1-5 are XRD patterns of powder samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively; all powder samples have different manganese doping amounts, but the shape of the diffraction peaks of the powders does not change significantly, and with the increase of manganese doping amount, the intensity of the diffraction peak at 2θ=28.62° shows a trend of first increasing and then decreasing.).

[0060] Figure 2SEM images of powder samples #1-1, #1-2, #1-3, #1-4, and #1-5 are given (SEM is for the purpose of characterizing the microscopic morphology of the material. The figure shows SEM images of powder samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively. All powders were photographed at 7000 times; the figure shows that the NPO powder particles are uneven in size and there is slight agglomeration. The average grain size of the powder shows a trend of first decreasing and then increasing with the increase of manganese doping amount. The average particle size is approximately 2.12, 1.70, 1.86, 2.01, and 1.95μm, respectively.).

[0061] Figure 3 XRD diagrams of ceramic samples #1-6, #1-7, #1-8, #1-9, and #1-10 (XRD is a technique that uses the diffraction effect of X-rays in crystalline materials to analyze the structure of materials, where the horizontal axis in the figure is the 2θ angle and the vertical axis is the relative intensity. In the figure, #1-6, #1-7, #1-8, #1-9, and #1-10 are XRD diagrams of ceramic samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively. The XRD spectrum of the amorphous sample shows a large peak. Relative to the XRD diffraction peak of the powder, the XRD diffraction peak of the ceramic moves toward the low-angle end, and the unit cell volume of the crystal increases.).

[0062] Figure 4 SEM images of ceramic samples #1-6, #1-7, #1-8, #1-9, and #1-10 are given. (SEM is used to characterize the microscopic morphology of materials. The figures show SEM images of ceramic samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively. All powders were photographed at 4000 times the magnification. There is no obvious grain morphology in the ceramics, but they are in a molten state. In this state, the grain boundaries become blurred and it is difficult to distinguish obvious grain outlines.)

[0063] Figure 5 This is the EDS image of a ceramic sample with a manganese doping level of 0.53wt% (EDS is used to analyze the types and contents of elemental components in the micro-region of the material. A total of Al, Sr, Sb, Ba, Ti, V, Sm, Mn, Bi and other elements were detected. Among them, Sm has the highest content, with a mass fraction of more than 30wt%; followed by Bi and Ti, with mass fractions between 10 and 30wt%; then Sr, Sb, and Ba, with mass fractions all below 10wt%; the smallest mass fractions are V, Al, and Mn, with mass fractions less than 1wt%.).

[0064] Figure 6 This is a characteristic curve diagram of the dielectric constant of ceramic samples changing with temperature (the horizontal axis in the dielectric constant diagram is temperature, and the vertical axis is dielectric constant. In the figure, #1-6, #1-7, #1-8, #1-9, and #1-10 are dielectric constant diagrams of ceramic samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively. Appropriate manganese doping has a significant effect on improving the high-temperature dielectric constant of NPO ceramics, and the maximum high-temperature dielectric constant reaches 1029.8.).

[0065] The main dielectric properties of the ceramic samples are shown in Table 1.

[0066] Table 1 Dielectric properties of ceramic samples #1-6, #1-7, #1-8, #1-9, #1-10

[0067]

[0068] In the table, #1-6, #1-7, #1-8, #1-9, and #1-10 are ceramic samples with manganese doping contents of 0.16wt%, 0.27wt%, 0.31wt%, 0.39wt%, and 0.53wt%, respectively. It can be concluded from the table that appropriate manganese doping has a significant effect on improving the room temperature dielectric constant of NPO ceramics. The dielectric constant of the ceramic sample with a manganese doping mass fraction of 0.31wt% is the largest, reaching 126.

[0069] Example 2

[0070] This embodiment is to prepare NPO ceramic materials by sintering ceramic powder with a manganese doping amount of 0.27wt% at different temperatures, wherein the sintering temperatures are 1200°C, 1230°C, and 1260°C, and the serial numbers of the samples sintered at different temperatures are respectively recorded as #2-1, #2-2, and #2-3; the specific steps of preparing NPO ceramic dielectric materials sintered at different temperatures with the same manganese doping amount by the present invention are as follows:

[0071] (1) Calculate the mass of various raw materials required according to the molecular formula and mass fraction, including but not limited to (CH 3 COO 2 Ba、Sm 2 O 3 、Bi 2 O 3 、TiO 2 , Additive V 2 O 5 , Sb 2 O 3 、SiO 2 , (CH3 COO 3 Al, (CH 3 COO 2 At least one of Sr, (CH 3 COO 2 Mn; weigh accurately with an electronic analytical balance. Add the weighed raw materials into a clean ball mill, and add ethanol, pure water and clean zirconia beads into the ball mill according to the mass ratio of ethanol: pure water: powder = 1:2:3, zirconia beads: powder = 3:1;

[0072] (2) Fix the ball mill jar to the ball mill and tighten the nut, adjust the speed to 400 r / min, and adjust the speed to 300 r / min after 30 minutes, and ball mill at a speed of 300 r / min for 10 hours;

[0073] (3) After planetary ball milling, the slurry is placed in an oven at 60°C to dry completely;

[0074] (4) The dried powder was transferred to a clean and dry crucible for pre-sintering. The heating rate was set to 2°C / min from room temperature to 500°C, kept at this temperature for 30 min, then heated to 900°C at 4°C / min, kept at this temperature for 1 h, then heated to 1000°C at 4°C / min, kept at this temperature for 2 h, and then cooled to room temperature;

[0075] (5) Pour the pre-burned powder into an agate mortar, add 3 drops of polyvinyl alcohol (PVA) at a ratio of 1 gram of powder, and grind in a clockwise direction until no large particles are left and the powder is fine and smooth;

[0076] (6) Weigh 0.5 g of the powder into a mold and press it into a uniform sheet with a diameter of 10 mm;

[0077] (7) The sintering temperatures were adjusted to 1200°C, 1230°C, and 1260°C, respectively. The heating rate during the sintering process was set to 2°C / min from room temperature to 500°C, kept at that temperature for 30 min, then heated to 900°C at 4°C / min, kept at that temperature for 1 h, then heated to the required sintering temperature at 4°C / min, kept at that temperature for 2 h, and cooled to room temperature to obtain three ceramic samples.

[0078] in, Figure 7XRD diagrams of ceramic samples #2-1, #2-2, and #2-3; (XRD is a technique that uses the diffraction effect of X-rays in crystalline materials to analyze the structure of materials, where the horizontal axis in the figure is the 2θ angle and the vertical axis is the relative intensity. In the figure, #2-1, #2-2, and #2-3 are XRD diagrams of ceramic samples sintered at 1200°C, 1230°C, and 1260°C, respectively, when the manganese doping is 0.27wt%. When the sintering temperature is 1230°C, it can be found that the signal intensity of the diffraction peak is significantly enhanced compared to the ceramics sintered at other temperature conditions.).

[0079] Figure 8 SEM images of ceramic samples #2-1, #2-2, and #2-3 are given (SEM is used to characterize the microscopic morphology of materials. The ceramic samples were photographed at 16000, 4000, and 16000 magnifications, respectively. There are obvious grains on the surface of ceramics sintered at 1200℃ and 1260℃, while the surface of ceramics sintered at 1230℃ is in a molten state. With the increase of sintering temperature, the number of large particles decreases and the grain distribution becomes more uniform.).

[0080] Fig. 9 The dielectric constant of the ceramic sample changes with temperature. (The horizontal axis in the dielectric constant graph is temperature, and the vertical axis is dielectric constant. In the figure, #2-1, #2-2, and #2-3 are dielectric constant graphs of ceramic samples sintered at 1200°C, 1230°C, and 1260°C, respectively, when the manganese doping is 0.27wt%. When the test temperature is below 250°C, the change in sintering temperature has little effect on the dielectric constant. In terms of temperature stability, the temperature stability of ceramics sintered at 1260°C is better than that of ceramics sintered at 1200°C and 1230°C. The higher the sintering temperature, the better the temperature stability of the ceramics.).

[0081] The main dielectric properties are shown in Table 2.

[0082] Table 2 Dielectric properties of ceramic samples #2-1, #2-2, #2-3

[0083]

[0084] #2-1, #2-2, and #2-3 in the table are the dielectric properties of ceramic samples sintered at 1200°C, 1230°C, and 1260°C, respectively, when the manganese doping amount is 0.27wt%. It can be seen from the table that when the mass fraction of manganese doping is 0.27wt%, the room temperature dielectric constant of the ceramic sintered at 1260°C is the largest, which is 124, and the dielectric loss is 0.0005.

[0085] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0086] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A NPO energy storage dielectric ceramic material, It is characterized in that In terms of mass percentage, the proportions of the components are as follows: the main component is 15-30% BaTiO 3 20-40% Sm 2 O 3 , 15-30% Bi 2 O 3 30-50% TiO 2 , 0.16-0.53% manganese oxide, additive 0.1-1.0% V 2 O 5 , 0.1-0.5% Sb 2 O 3 , 0.1-0.5% SiO 2 , 0.1-0.5% Al 2 O 3 , 1.5-2.0% SrO.

2. The method for preparing the NPO energy storage dielectric ceramic material according to claim 1, It is characterized in that The room temperature dielectric constant of the NPO energy storage dielectric ceramic material is 120-125.

3. The method for preparing the NPO energy storage dielectric ceramic material according to claim 1, It is characterized in that The room temperature dielectric loss of the NPO energy storage dielectric ceramic material is 0.0003-0.0010.

4. A method for preparing the NPO energy storage dielectric ceramic material according to any one of claims 1 to 3, It is characterized in that Specifically: Firstly, the required raw materials are weighed according to the mass fraction ratio, and then the manganese-doped NPO powder is prepared by a solid phase reaction method, and finally the manganese-doped NPO energy storage dielectric ceramic material is prepared by sintering.

5. The method for preparing the NPO energy storage dielectric ceramic material according to claim 4, It is characterized in that The specific steps are as follows; Step 1, calculate the mass of various raw materials required according to the mass fraction ratio and weigh them, then add the weighed raw materials into a grinder, and add a certain proportion of ethanol, water and zirconium oxide balls into the grinder; Step 2, after grinding for the first time, reduce the speed and ball mill for the second time; Step 3: Dry the ground slurry until it is completely dry; Step 4: pre-burn the dried powder for a certain period of time, and then take it out for use after the powder temperature drops to room temperature; Step 5: Pour the pre-burned powder into a mortar, add a certain amount of PVA and grind until the powder is fine and smooth, then stop grinding; Step 6: Weigh a certain amount of ground powder, pour it into a corresponding mold after granulation, press it into thin slices of a certain diameter and uniform texture, and then put it into a marked ziplock bag for later use; Step 7: Sinter the obtained slices to prepare manganese-doped NPO energy storage dielectric ceramic materials.

6. The method for preparing the NPO energy storage dielectric ceramic material according to claim 5, It is characterized in that In step 1, the raw materials include but are not limited to (CH 3 COO 2 Ba、Sm 2 O 3 、Bi 2 O 3 、TiO 2 , the additive is V 2 O 5 , Sb 2 O 3 、SiO 2 , (CH 3 COO 3 Al, (CH 3 COO 2 At least one of Sr, (CH 3 COO 2 Mn.

7. The method for preparing the NPO energy storage dielectric ceramic material according to claim 5, It is characterized in that In step 1, the mass ratio of ethanol:pure water:powder:zirconia beads is 1:2:3:

9.

8. The method for preparing the NPO energy storage dielectric ceramic material according to claim 5, It is characterized in that In step 6, the thickness of the sheet is 1.30-1.60 mm.

9. The method for preparing the NPO energy storage dielectric ceramic material according to claim 5, It is characterized in that In step 7, the slice is kept at 1200-1260° C. for 0.5-2 h and sintered to form NPO energy storage dielectric ceramic material.

10. An application of the NPO energy storage dielectric ceramic material prepared by the preparation method according to any one of claims 4 to 9, It is characterized in that The NPO energy storage dielectric ceramic material is used in, but not limited to, preparing oscillators, resonators, and high-frequency circuits.

Citation Information

Patent Citations

  • Microwave dielectric ceramic and preparation method thereof

    CN108863347A

  • Lead-free barium titanate-based ceramic material with high energy storage performance and preparation method thereof

    CN115215648A

  • Barium titanate-based energy storage ceramic as well as preparation method and application thereof

    CN117602933A

  • Dielectric ceramic composition, method for manufacturing the same, and multilayer capacitor

    JP2003267778A