A microwave dielectric ceramic with near-zero resonant frequency temperature coefficient and preparation method thereof
By introducing Zr4+ ions into Sm2TiO5 ceramics and controlling the phase change process, the resonance frequency temperature coefficient of microwave dielectric ceramics is nearly zero, solving the problem of difficult balance of performance indicators in the existing technology, and significantly improving the microwave dielectric performance of the material. Suitable for a variety of microwave devices.
Patent Information
- Application Number
- CN202411223432.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Existing microwave dielectric ceramic materials have difficulty in balancing performance indicators between low dielectric constant, high Q value and near zero resonant frequency temperature coefficient (τf), especially in Re2TiO5 systems, the τf value of orthogonal and cubic phases. On the contrary, it is difficult to achieve near zero τf value through phase transition induction.
By performing Zr4+ ion replacement in Sm2TiO5, Sm2Ti1-xZrxO5 ceramics are designed to regulate the phase change process to achieve near zero τf value. The specific steps include wet ball milling, prefiring, bonding and sintering, and controlling the Zr content at 0.20≤x≤0.30 To induce orthogonal-cube phase transition, it reaches a near zero τf value.
成功实现了钛酸盐微波介质陶瓷的谐振频率温度系数近零,显著提高了材料的微波介电性能,适用于各种微波器件的制造,具有工业应用价值,并为开发更优性能的微波介质 Ceramics opens up new paths.
Smart Images

Figure CN118754654B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric ceramic materials, and in particular relates to a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient and a preparation method thereof. Background Art
[0002] Microwave dielectric ceramics (MWDC) refer to functional ceramics that play a key role as dielectric materials in circuits within the microwave frequency band (300MHz to 300GHz). These materials are indispensable in modern communication systems and are widely used in microwave components such as resonators, filters, and dielectric waveguide circuits. They are crucial to the development of technology fields such as radar, mobile communication equipment, and global positioning system (GPS) antennas.
[0003] In the evolution of high-speed communication networks, microwave dielectric ceramics (MWDC) are key components, and their development direction is to have low dielectric constant (ε r ), high Q value (Q×f) and near-zero resonant frequency temperature coefficient (τ f However, there are mutual influences and constraints between these performance indicators in the material system. For example, materials with high dielectric constants are often accompanied by higher dielectric losses, while materials with low dielectric constants may produce non-zero negative τ f Therefore, in order to achieve the optimal performance of microwave components, an ideal balance between these performance parameters must be achieved in the material system.
[0004] In the binary Re2O3-TiO2 system, Re2TiO5 compounds have attracted much attention due to their adjustable chemical composition and polymorphic structural transformations. These structural transformations cover orthorhombic, hexagonal and cubic forms determined by the size of the rare earth cations (YF Shepelev, MA Petrova, Crystal structures of Ln2TiO5(Ln = Gd, Dy)polymorphs, Inorg. Mater. 44 (2008) 1354-1361). Larger rare earth ions tend to form orthorhombic crystals, while smaller ions tend to form cubic crystals with higher symmetry. Medium-sized ions may show multiple tendencies of orthorhombic, hexagonal or cubic crystals, or coexist in multiple crystal forms under specific sintering conditions. These structural changes are also related to the coordination environment and / or deformation of the polyhedron formed by the B-site ions bonding with adjacent oxygen atoms. Therefore, the relationship between the crystal structure of Re2TiO5 compounds and their A / B-site ion radius ratio provides an important basis for accurately predicting their crystal structures.
[0005] At present, the research on the microwave dielectric properties of Re2TiO5 ceramics is relatively limited. It is known that orthogonal Re2TiO5 (Re = Sm, Eu) ceramics exhibit excellent microwave dielectric properties. r Between 14.40 and 15.34, with Q×f as high as 17795 to 21000 GHz, and negative τ of -13 to -10 ppm / °C f In contrast, cubic Re2TiO5 (Re = Er, Lu) exhibits a positive τ of about +20 ppm / ℃. f value (GB Zhu, DQ Chen, XW Zhu, et al. Re2TiO5: Special dielectrictitanates exhibiting abnormally low permittivity and a positivecoefficient ofresonance frequency, J. Am. Ceram. Soc. 107 (2023) 2029-2039). In order to adjust τ f value to near zero, the conventional approach is to have the opposite τ f The second phase material with the same value is added into the main phase. Since the orthorhombic phase and cubic phase of Re2TiO5 series ceramics have opposite τ f value, which makes the phase transition induced development with near-zero τ f High-quality Re2TiO5 microwave dielectric ceramics become possible.
[0006] Therefore, the present invention proposes a composition design strategy to achieve phase transition by ion substitution at the B site of Sm2TiO5, aiming to adjust its microwave dielectric properties, especially to explore the near-zero τ f dielectric ceramic materials. Summary of the invention
[0007] In order to achieve the goal of having a near-zero resonant frequency temperature coefficient of a titanate microwave dielectric ceramic, the present invention provides a microwave dielectric ceramic having a near-zero resonant frequency temperature coefficient and a preparation method thereof.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient, whose chemical composition is Sm2Ti 1-x Zr x O5, where 0.20≤x≤0.30.
[0010] The preparation method of the microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient comprises the following steps:
[0011] (1) The original powders of Sm2O3, TiO2 and ZrO2 are mixed into Sm2Ti 1-x Zr x The composition of O5 is weighed and prepared, the original powders are mixed and wet ball milled, and the ball mill slurry is dried to obtain a mixture A;
[0012] (2) pre-calcining the mixture A obtained in step (1) to obtain a powder;
[0013] (3) wet-milling the powder obtained in step (2), and drying the milled slurry to obtain a mixture B;
[0014] (4) adding a binder to the mixture B obtained in step (3), granulating the mixture, sieving the mixture, and pressing the mixture into a green body;
[0015] (5) Debinding and sintering the green body obtained in step (4) to obtain titanate microwave dielectric ceramics.
[0016] Furthermore, in step (1) and step (3), the wet ball milling time is 6 hours, the medium of the wet ball milling is anhydrous ethanol, the ball milling speed is 300 r / min, and the rotation direction is reversed every 60 minutes; the ball milling slurry drying temperature is 120°C.
[0017] Furthermore, in step (2), the pre-burning temperature is 1150-1250°C and the time is 2-6 hours;
[0018] Preferably, in step (2), the pre-burning temperature is 1200° C. and the time is 4 hours.
[0019] Furthermore, in step (4), the binder is a polyvinyl alcohol solution with a mass concentration of 5%, the mass of the binder does not exceed 3% of the mass of the mixture B, and a 60-120 mesh sieve is used for sieving.
[0020] Furthermore, in step (5), the debinding temperature is 550°C and the holding time is 6 hours; the sintering is carried out in an air atmosphere, the sintering temperature is 1375-1475°C, and the holding time is 4 hours.
[0021] Preferably, in step (5), the sintering temperature is 1425°C.
[0022] Preferably, in step (1), the purity of the original powder is 99.9%.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention realizes near-zero temperature coefficient of resonant frequency of titanate ceramics by regulating phase change. The specific method is as follows: 1-x Zr x Precise doping of Zr in O5-based titanate microwave dielectric ceramics 4+ ions, effectively inducing and controlling the phase change process, when the x value is between 0.20 and 0.30, the microwave dielectric ceramics exhibit a near-zero τ f Value properties.
[0025] 2. The microwave dielectric ceramics prepared by the method of the present invention have the excellent performance of a resonant frequency temperature coefficient of near zero, and can be widely used in the manufacture of various dielectric substrates, resonators, filters and other microwave devices, and have significant industrial application value.
[0026] 3. The phase change strategy designed in the present invention is not only to design a near-zero τ f It provides a new method for microwave dielectric ceramics and opens up a promising path for developing advanced microwave dielectric ceramic materials with better performance and higher reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The microwave dielectric ceramic Sm2Ti prepared in Example 1 1-x Zr x Comparison chart of XRD (X-ray diffraction pattern) and SEM image (scanning electron microscope image) of O5 (x=0.20), where a is the XRD pattern and b is the SEM image.
[0028] Figure 2 The microwave dielectric ceramic Sm2Ti prepared in Example 2 1-x Zr x XRD comparison chart and SEM image of O5 (x = 0.30), where a is the XRD chart and b is the SEM image.
[0029] Figure 3 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 1 1-x Zr x XRD comparison diagram of O5 (x=0.02).
[0030] Figure 4 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 2 1-x Zr x XRD comparison chart of O5 (x=0.05).
[0031] Figure 5 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 3 1-x Zr x XRD comparison diagram of O5 (x=0.10).
[0032] Figure 6 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 4 1-x Zr x XRD comparison diagram of O5 (x=0.40).
[0033] Figure 7 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 5 1-x Zr x XRD comparison diagram of O5 (x=0.45).
[0034] Figure 8 The microwave dielectric ceramic Sm2Ti prepared in Comparative Example 6 1-x Zr x XRD comparison diagram of O5 (x=0.55). DETAILED DESCRIPTION
[0035] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0036] The present invention proposes a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient and a preparation method thereof, and achieves a near-zero resonant frequency temperature coefficient of titanate ceramics by regulating phase change. The microwave dielectric ceramic involved in the method has a chemical formula of Sm2Ti 1-x Zr x O5, select Zr 4+ As a replacement ion at the Ti site, by 1-x Zr x Precise doping of Zr in O5 4+ ions, design and manufacture a series of Sm2Ti 1-x Zr xO5 ceramic samples, where x takes values of 0.02, 0.05, 0.10, 0.20, 0.30, 0.40, 0.45, and 0.55, respectively, change the A / B ratio by adjusting the Zr content, cross the orthorhombic-cubic phase transition, effectively induce and control the phase transition process, and thus achieve the goal of near-zero temperature coefficient of resonant frequency of microwave dielectric ceramics.
[0037] The specific preparation method comprises the following steps:
[0038] (1) The original powders of Sm2O3, TiO2 and ZrO2 with a purity of more than 99.9% (weight percentage) are mixed into Sm2Ti 1- x Zr x The ingredients were weighed and prepared in a molar ratio of 1:1 to 5:1, and the prepared original powders were mixed and added into a ball mill. The wet ball milling was carried out for 6 hours. The medium for the wet ball milling was anhydrous ethanol. The ball milling speed was 300 r / min, and the rotation was reversed every 60 minutes. The ball milled slurry was dried at 120°C to obtain a mixture A.
[0039] (2) Pre-calcining the mixture A obtained in step (1) to obtain powder; wherein the pre-calcining temperature is 1150-1250°C and the holding time is 2-6 hours. The present invention adopts a pre-calcining temperature of 1200°C and a holding time of 4 hours.
[0040] (3) The powder obtained in step (2) was wet-milled for 6 h. The medium for wet-milling was anhydrous ethanol. The ball milling speed was 300 r / min, and the rotation direction was reversed every 60 min. The ball milled slurry was dried at 120° C. to obtain a mixture B.
[0041] (4) Add a binder to the mixture B obtained in step (3), granulate, screen, and press into a green body. The binder is a polyvinyl alcohol solution with a mass concentration of 5%, and the mass of the binder does not exceed 3% of the mass of the mixture B, preferably 3%. Use a 60-120 mesh screen for screening. Use a powder tablet press to press the granulated and screened mixture B into a cylindrical green body with a diameter of 11-12 mm and a thickness of 5-6 mm.
[0042] (5) Debinding and sintering the green body obtained in step (4) to obtain titanate microwave dielectric ceramics. Debinding and sintering are both carried out in a muffle furnace; the debinding temperature is 550°C, the holding time is 6 hours, and the heating rate is 1.5°C / min; sintering is carried out in an atmospheric atmosphere, the sintering temperature is 1375~1475°C, the holding time is 4 hours, and the optimal sintering temperature is 1425°C.
[0043] The dielectric properties of microwave dielectric ceramics are determined by intrinsic factors and extrinsic factors. The appropriate sintering temperature can eliminate the influence of extrinsic factors on the properties to a certain extent. It is generally believed that highly densified ceramic samples have the best dielectric properties, while the presence of microscopic pores will impair the dielectric properties. In the present invention, when the value of x is the same, the target product Sm2Ti cannot be synthesized if the sintering temperature is lower than 1375℃. 1-x Zr x O5, when the sintering temperature is between 1375 and 1425°C, the volume density of the ceramic sample increases with the increase of temperature, and when the sintering temperature is higher than 1425°C, the volume density of the ceramic sample decreases with the continuous increase of temperature, that is, the ceramic sample sintered in the atmosphere at 1425°C for 4 hours has the highest degree of densification and the best comprehensive dielectric properties. When x of the present invention takes values of 0.02, 0.05, 0.10, 0.20, 0.30, 0.40, 0.45, and 0.55, the performance index values of the ceramic samples at different sintering temperatures are shown in Table 1.
[0044] Table 1 Performance index values of ceramic samples at different sintering temperatures
[0045]
[0046] All the raw materials used above were purchased from commercial sources.
[0047] The technical solution of the present invention is further illustrated by the following examples and comparative examples.
[0048] Example 1
[0049] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.20).
[0050] Its X-ray diffraction (XRD) pattern and scanning electron microscope (SEM) image are shown in Figure 1 After sintering at 1425℃, the diffraction peak of the ceramic material is simultaneously with that of the orthorhombic phase Sm2TiO5 (see Figure 1 Figure 00-022-1306) and cubic phase Sm2TiO5 (see Figure 1 00-034-1333), which shows that under this sintering condition, Sm2Ti 1-x Zr x O5 (x = 0.20) ceramics exhibit a dual crystal structure of orthorhombic and cubic phases. SEM images further reveal that the ceramic grains are closely arranged, with clear grain boundaries and no obvious pores, which further confirms the high-quality sintering state of the material. In particular, the τ fThe value reached -3.8 ppm / ℃, which is close to zero, which shows that the present invention is effective in achieving near-zero τ f Significant effect on value.
[0051] Example 2
[0052] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.30).
[0053] Its X-ray diffraction pattern and scanning electron microscope image are shown in Figure 2 After sintering at 1425℃, the diffraction peak of the ceramic material is simultaneously with that of the orthorhombic phase Sm2TiO5 (see Figure 2 Figure 00-022-1306) and cubic phase Sm2TiO5 (see Figure 2 00-034-1333), which shows that under this sintering condition, Sm2Ti 1-x Zr x O5 (x = 0.30) ceramics exhibit a dual crystal structure of orthorhombic and cubic phases. SEM images further reveal that the ceramic grains are closely arranged, with clear grain boundaries and no obvious pores, which further confirms the high-quality sintering state of the material. In particular, the τ f The value reached +1.6 ppm / ℃, which is close to zero, which shows that the present invention is effective in achieving near-zero τ f Significant effect on value.
[0054] Comparative Example 1
[0055] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.02).
[0056] pass Figure 3 The X-ray diffraction analysis shown in Figure 2 shows that the sample sintered at 1425 °C only shows the orthorhombic phase Sm2TiO5 (see Figure 3 The diffraction peaks of Sm2TiO2 matched those of Figure 00-022-1306 in Figure 00-022-1306, and no other phases were detected. This indicates that at this sintering temperature, the material formed a single orthorhombic crystal structure. It is worth noting that Sm2Ti 1-x Zr x τ of O5 (x=0.02) ceramics f The value is -16.0 ppm / ℃, which shows that it has a significant non-near-zero negative value, which is consistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0057] Comparative Example 2
[0058] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.05).
[0059] pass Figure 4 The X-ray diffraction analysis shown in Figure 2 shows that the sample sintered at 1425 °C only shows the orthorhombic phase Sm2TiO5 (see Figure 4 The diffraction peaks of Sm2TiO2 matched those of Figure 00-022-1306 in Figure 00-022-1306, and no other phases were detected. This indicates that at this sintering temperature, the material formed a single orthorhombic crystal structure. It is worth noting that Sm2Ti 1-x Zr x τ of O5 (x=0.05) ceramics f The value is -19.7 ppm / ℃, which shows that it has a significant non-near-zero negative value, which is consistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0060] Comparative Example 3
[0061] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.10).
[0062] pass Figure 5 The X-ray diffraction analysis shown in the figure shows that the diffraction peaks of the sample sintered at 1425°C can be simultaneously with those of the orthorhombic phase Sm2TiO5 (see Figure 5 Figure 00-022-1306) and cubic Sm2TiO5 (see Figure 5 This shows that under this sintering condition, Sm2Ti 1-x Zr x O5 (x = 0.10) ceramics exhibit a dual crystal structure of orthorhombic and cubic phases. However, the τ f The value is -15.9 ppm / ℃, showing a non-near-zero negative value, which is inconsistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0063] Comparative Example 4
[0064] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.40).
[0065] pass Figure 6The X-ray diffraction analysis shown in the figure shows that the diffraction peaks of the sample sintered at 1425°C can be simultaneously with those of the orthorhombic phase Sm2TiO5 (see Figure 6 00-022-1306) and cubic Sm2TiO5 (see Figure 6 This shows that under this sintering condition, Sm2Ti 1-x Zr x O5 (x = 0.40) ceramics exhibit a dual crystal structure of orthorhombic and cubic phases. However, the τ f The value is +9.8 ppm / ℃, showing a non-near-zero positive value, which is consistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0066] Comparative Example 5
[0067] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.45).
[0068] pass Figure 7 The X-ray diffraction analysis shown in the figure shows that the diffraction peaks of the sample sintered at 1425°C can be simultaneously with those of the orthorhombic phase Sm2TiO5 (see Figure 7 Figure 00-022-1306) and cubic phase Sm2TiO5 (see Figure 7 This shows that under this sintering condition, Sm2Ti 1-x Zr x O5 (x = 0.45) ceramics exhibit a dual crystal structure of orthorhombic and cubic phases. However, the τ f The value is +18.6 ppm / ℃, showing a non-near-zero positive value, which is inconsistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0069] Comparative Example 6
[0070] The microwave dielectric ceramic Sm2Ti was prepared by the above preparation method. 1-x Zr x O5 (x=0.55).
[0071] pass Figure 8 The X-ray diffraction analysis shown in Figure 2 shows that the sample sintered at 1425 °C only shows the cubic phase Sm2TiO5 (see Figure 800-034-1333) in the sintering temperature, and no other phases were detected. This indicates that the material forms a single cubic crystal structure at this sintering temperature. 1-x Zr x τ of O5 (x=0.55) ceramics f The value is +22.4 ppm / ℃, which shows that it has a significant non-near-zero positive value, which is consistent with the near-zero τ pursued by the present invention. f The value targets vary.
[0072] In Example 1 and Example 2, the prepared ceramic material successfully achieved a near-zero τ f In contrast, the ceramic materials prepared in Comparative Examples 1 to 6 show non-zero τ f These results fully demonstrate the feasibility and effectiveness of the method of the present invention for regulating the resonant frequency temperature coefficient of titanate microwave dielectric ceramics to near zero through phase change.
[0073] The microwave dielectric properties of the dielectric ceramics prepared in the above Examples 1-2 and Comparative Examples 1-6 were tested respectively. The test results are shown in Table 2.
[0074] Table 2 Sm2Ti 1-x Zr x Microwave Dielectric Properties of O5 Microwave Dielectric Ceramics
[0075]
[0076] It can be seen from Table 2 that the ε of the microwave dielectric ceramic materials prepared by the above eight different x values r The value reaches 14.30 ~ 23.18, the Q×f value reaches 14828~22300 GHz, τ f The value reaches -19.7~+22.4, which has excellent microwave dielectric properties. In particular, when 0.20≤x≤0.30, it reaches a near-zero τ of -3.8 ~+1.6 ppm / ℃ f value.
[0077] Based on the above test results, it can be seen that when the x value is 0.02 or 0.05, the doped Zr 4+ The ions are relatively small, and the XRD pattern of the obtained ceramic sample is consistent with the diffraction peak of the orthorhombic phase Sm2TiO5 (see Figure 3 , Figure 4 00-022-1306 in Figure 1) is completely consistent, indicating that Sm2Ti 1-x Zr xO5 ceramics maintain the same orthorhombic crystal structure as the matrix Sm2TiO5. As the x value gradually increases to 0.10, 0.20, 0.30, 0.40 or 0.45, in addition to the diffraction peak of the orthorhombic phase in the XRD pattern (see Figure 1~2 , Figures 5 to 7 In addition to the diffraction peaks matching those of cubic phase Sm2TiO5 (see Figure 1~2 , Figures 5 to 7 00-034-1333 in Figure 1), which shows that Sm2Ti 1-x Zr x O5 ceramics show a dual-phase coexistence state of orthorhombic phase and cubic phase. When the x value is further increased to 0.55, the doped Zr 4+ The ions are relatively abundant, the orthorhombic phase disappears completely, and the ceramic is completely transformed into a cubic phase structure. 1-x Zr x O5 ceramics are cubic single phase. The above phase transition strategy realizes Sm2Ti 1-x Zr x O5 ceramic τ f The value gradually changes from the negative value of the orthorhombic phase to the positive value of the cubic phase. In particular, when the x value is 0.20 and 0.30, the ceramic sample exhibits a near-zero τ of -3.8 ppm / ℃ and +1.6 ppm / ℃, respectively. f This fully demonstrates the feasibility and effectiveness of the phase change strategy in the present invention in regulating the temperature coefficient of the resonant frequency.
[0078] The τ f Microwave dielectric ceramic materials with near-zero values can be widely used in the manufacture of various microwave devices such as dielectric substrates, resonators and filters, and have significant industrial application value.
[0079] The phase change strategy designed in the present invention is not only to design a near-zero τ f It provides a new method for microwave dielectric ceramics and opens up a promising path for developing advanced microwave dielectric ceramic materials with better performance and higher reliability.
[0080] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient, characterized in that: Its chemical composition is Sm2Ti 1- x Zr x O5, where 0.20≤x≤0.
30.
2. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 1, characterized in that: The following steps are involved: (1) The original powders of Sm2O3, TiO2 and ZrO2 are mixed into Sm2Ti 1-x Zr x The composition of O5 is weighed and prepared, the original powders are mixed and wet ball milled, and the ball mill slurry is dried to obtain a mixture A; (2) pre-calcining the mixture A obtained in step (1) to obtain a powder; (3) wet-milling the powder obtained in step (2), and drying the milled slurry to obtain a mixture B; (4) adding a binder to the mixture B obtained in step (3), granulating the mixture, sieving the mixture, and pressing the mixture into a green body; (5) Debinding and sintering the green body obtained in step (4) to obtain microwave dielectric ceramics.
3. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 2, characterized in that: In the steps (1) and (3), the wet ball milling time is 6 hours, the medium of the wet ball milling is anhydrous ethanol, the ball milling speed is 300 r / min, and the rotation direction is reversed every 60 minutes; the ball milling slurry is dried at a temperature of 120°C.
4. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 2, characterized in that: In the step (2), the pre-burning temperature is 1150-1250° C. and the time is 2-6 hours.
5. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 4, characterized in that: In the step (2), the pre-burning temperature is 1200° C. and the time is 4 hours.
6. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 2, characterized in that: In the step (4), the binder is a polyvinyl alcohol solution with a mass concentration of 5%, the mass of the binder does not exceed 3% of the mass of the mixture B, and the sieving uses a 60-120 mesh screen.
7. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 2, characterized in that: In the step (5), the debinding temperature is 550°C and the time is 6 hours; the sintering is carried out in an air atmosphere, the sintering temperature is 1375-1475°C and the time is 4 hours.
8. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 7, characterized in that: In the step (5), the sintering temperature is 1425°C.
9. The method for preparing a microwave dielectric ceramic with a near-zero resonant frequency temperature coefficient according to claim 2, characterized in that: In the step (1), the purity of the original powder is 99.9%.
Citation Information
Patent Citations
Preparation method of microwave dielectric ceramic material
CN103864420A
Composite tantalate microwave dielectric ceramic with near-zero frequency temperature coefficient
CN105060892A
Microwave dielectric material with near-zero temperature coefficient of resonance frequency
CN110668814A
Microwave dielectric ceramic with low sintering temperature and adjustable dielectric property
CN112250441A
Microwave dielectric ceramic material with low expansion coefficient, and preparation method thereof
CN112745106A