Ceramic matrix composite material photocuring forming method
By forming a protective layer by UV curing on the surface of ceramic matrix composite materials, combined with high-temperature cracking process, the problem of pores and defects in the manufacturing of traditional ceramic matrix composite materials is solved, the process flow is simplified, the material density and performance are improved, and efficient Densification process.
Patent Information
- Application Number
- CN202410848724.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
In the traditional ceramic matrix composite manufacturing process, the overflow and density increase of small molecules during the precursor cracking process lead to volume shrinkage, formation of pores and defects, affecting material properties, and the curing process is time-consuming and complex.
The photo-curing molding method of ceramic matrix composite materials is adopted, including dipping process, ultraviolet light curing process and high-temperature cracking process. The ultraviolet light precursor solution is sprayed on the surface of the composite material for ultraviolet light curing to form a protective layer, reduce the volatilization of small molecules, and Cracking is performed at high temperatures to simplify the process.
The curing process is simplified, manufacturing efficiency is improved, energy consumption is reduced, the thickness of the protective layer is controlled to adjust the degree of material densification, porosity is reduced, and material density and performance are improved.
Smart Images

Figure CN118754690A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of ceramic matrix composite material manufacturing, and in particular to a photocuring molding method of ceramic matrix composite material. Background Art
[0002] Continuous fiber reinforced ceramic matrix composites have many advantages such as good mechanical properties, high temperature resistance, strong oxidation resistance and ablation resistance, so it has great potential for application as a high temperature resistant structural material in the fields of aviation, aerospace industry and energy industry. Continuous fiber reinforced ceramic matrix composites have become the preferred material solution for the thermal structure of the new generation of near-space aircraft.
[0003] At present, ceramic-based composite materials are mostly manufactured by PIP process. Under certain temperature and pressure, carbon fiber preforms are used as the skeleton, organic precursor solutions are used for impregnation, cross-linking and curing, and high-temperature pyrolysis is carried out under the protection of inert gas to convert the precursor into a ceramic matrix. The PIP process has low cost, simple equipment requirements, and the precursor molecules can be designed, so that large and complex-shaped components can be manufactured. However, due to the overflow of small molecules during the pyrolysis of traditional precursors and the increase in the density of pyrolysis products, the volume of the precursor shrinks after pyrolysis, and pores and defects are formed during the material manufacturing process, which affects the performance of ceramic-based composite materials and becomes the main challenge faced by PIP in the manufacture of ceramic-based composite materials. In order to obtain a high-density composite material, it is necessary to repeat the "impregnation-curing-pyrolysis" process for several cycles to obtain a dense ceramic-based composite material. After the impregnation process of the ceramic-based composite material, it is necessary to add metal tooling on the surface of the composite material for high-temperature curing treatment. After the curing process is completed, it is replaced with graphite tooling for high-temperature pyrolysis. In this process, the curing process is time-consuming and the process is complicated. Summary of the invention
[0004] The present application provides a method for photocuring molding of ceramic-based composite materials, the purpose of which is to provide an alternative molding solution for ceramic-based composite materials, which can overcome the shortcomings of existing ceramic-based composite material curing process technology.
[0005] In a first aspect, a method for photocuring of a ceramic matrix composite material is provided, comprising:
[0006] Impregnation process: the fiber preform is immersed in an immersion barrel filled with a ceramic precursor impregnation matrix solution. After the immersion is completed, the preform is taken out of the immersion barrel and the excess impregnation matrix on the surface is scraped off;
[0007] UV curing process: spray the prepared UV precursor solution on the surface of the impregnated composite material, irradiate the composite material surface with UV light to form a protective layer on the composite material surface, and finally place the composite material in a graphite tooling;
[0008] High temperature cracking process: The graphite tooling containing the composite material is loaded into a high temperature furnace and subjected to high temperature cracking according to the high temperature cracking system to finally obtain a ceramic-based composite material.
[0009] In combination with the first aspect, in certain implementations of the first aspect, the UV curing process satisfies at least one of the following:
[0010] UV irradiation is performed at 0.1 cm to 10 cm on the surface of the composite material;
[0011] The intensity of UV light is 30-80mW / cm 3 ;
[0012] The irradiation time is 2-30min;
[0013] The irradiation angle is -45°~+45°;
[0014] The number of times of spraying the ultraviolet light precursor solution is controlled within 3-20 times.
[0015] In combination with the first aspect, in certain implementations of the first aspect, the thickness of the protective layer obtained by UV curing is 30-600 μm.
[0016] In combination with the first aspect, in certain implementations of the first aspect, the ceramic-based composite material is finally obtained for use in thermal insulation components of aircraft, and the thickness of the protective layer is 30-150 μm.
[0017] In combination with the first aspect, in certain implementations of the first aspect, the ceramic-based composite material is finally obtained for use in thermal protection structural components of an aircraft, and the thickness of the protective layer is 150-600 μm.
[0018] In combination with the first aspect, in certain implementations of the first aspect, the impregnation matrix solution includes at least one of the following organic precursor solutions: polycarbosilane, polyborosilazane, and polysilazane.
[0019] In combination with the first aspect, in certain implementations of the first aspect, the fiber used in the fiber preform includes at least one of the following: carbon fiber, silicon carbide fiber, Al-containing ceramic fiber, Hf-containing ceramic fiber, Zr-containing ceramic fiber, Ti-containing ceramic fiber.
[0020] In combination with the first aspect, in certain implementations of the first aspect, the ultraviolet light precursor is a resin containing an acrylic monomer.
[0021] In combination with the first aspect, in certain implementations of the first aspect, the ultraviolet light precursor includes at least one of the following: a SiC ceramic precursor containing an acrylic group, a SiBCN ceramic precursor containing an acrylic group, and an acrylic resin.
[0022] In combination with the first aspect, in certain implementations of the first aspect, the high-temperature cracking system includes two stages. In the first stage, the composite material is heated to 150-350°C at a heating rate of 2-15°C / min and kept warm for 1-4h. In the second stage, the composite material is heated to 800-1100°C at a heating rate of 5-10°C / min.
[0023] In combination with the first aspect, in certain implementations of the first aspect, the manufacturing steps of the ceramic-based composite material include multiple process rounds, the multiple process rounds include process round A and process round B, process round A is an impregnation process-UV light curing process-high temperature cracking process, and process round B is an impregnation process-thermal curing process-high temperature cracking process; process round B is performed before process round A.
[0024] In combination with the first aspect, in certain implementations of the first aspect, the thermal curing process includes: placing the impregnated composite material into a metal tooling, placing it in an oven and curing it at 300-400°C for 2-4 hours, and after the thermal curing process is completed, taking the composite material out of the oven and re-loading it into the graphite tooling.
[0025] In combination with the first aspect, in certain implementations of the first aspect, process round A is executed after process round B is fully executed, and process round A is used at a stage where the weight gain rate of the impregnated substrate is less than 10%.
[0026] In combination with the first aspect, in certain implementations of the first aspect, process round B is executed 2 to 4 times; and process round A is executed 1 to 4 times.
[0027] In combination with the first aspect, in certain implementations of the first aspect, after the process round B is fully executed, the density of the composite material is greater than 1.3 g / cm 3 .
[0028] In combination with the first aspect, in certain implementations of the first aspect, after the process round B is fully executed, the final porosity of the composite material is 5-30%.
[0029] In a second aspect, a ceramic-based composite material is provided, wherein the ceramic-based composite material is prepared by a method as described in any one of the implementations of the first aspect.
[0030] In a third aspect, an aircraft is provided, comprising a ceramic-based composite material as described in any one of the implementations of the second aspect, wherein the ceramic-based composite material is applied to a thermal insulation component or a heat-resistant structural component of the aircraft.
[0031] Compared with the prior art, the solution provided by this application includes at least the following beneficial technical effects:
[0032] (1) The present invention simplifies the curing process and only manufactures a protective layer on the surface of the composite material by UV curing of the precursor, thereby preventing the impregnated matrix from overflowing.
[0033] (2) The present invention manufactures a protective layer by ultraviolet curing, thereby reducing the volatilization of small molecules in the impregnated matrix during the high-temperature cracking process of the composite material and improving the manufacturing efficiency of the composite material.
[0034] (3) The protective layer manufactured by the present invention can be cured by ultraviolet light, with low weight loss rate during curing, simple curing process, short curing time and low energy consumption.
[0035] (4) The protective layer manufactured by the present invention can effectively control the thickness of the protective layer by adjusting the type of sprayed precursor and the number of spraying times, thereby controlling the volatilization rate of the small molecules impregnated into the matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the TG diagram of the protective layer after curing.
[0037] Figure 2 This is the SEM image of the protective layer after curing.
[0038] Figure 3 This is a graph showing the relationship between the irradiation intensity and the degree of curing of the photocurable precursor. DETAILED DESCRIPTION
[0039] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0040] The present invention relates to a photocuring molding process for a ceramic-based composite material, wherein the composite material manufacturing process comprises an impregnation process, an ultraviolet light curing process and a high-temperature cracking process. The impregnation process, the ultraviolet light curing process and the high-temperature cracking process can be performed cyclically to obtain a dense ceramic-based composite material.
[0041] (1) Impregnation process
[0042] The fiber preform is immersed in a soaking barrel filled with a ceramic precursor impregnation matrix solution. After the soaking is completed, the preform is taken out of the soaking barrel and the excess impregnation matrix on the surface is scraped off.
[0043] (2) UV curing process
[0044] The prepared UV precursor solution is sprayed on the surface of the impregnated composite material, and then according to a certain UV curing system, UV light of a certain intensity is irradiated on the surface of the composite material for a certain time, and finally the composite material is placed in a graphite tooling.
[0045] After UV-curing ceramic precursors are irradiated with UV light, free radicals trigger the unsaturated groups in the precursors to undergo cross-linking and curing reactions, forming a cured product with a certain degree of cross-linking, that is, forming a protective layer on the surface of the composite material. The cured product is basically infusible at 300°C (e.g. Figure 1 As shown, at a light intensity of 30W / cm 3 The weight loss of the cured product obtained by irradiating the precursor under ultraviolet light for 5 minutes before 300°C is less than 6wt%. In addition, after the protective layer is made of ultraviolet light-cured precursor, the small molecules of the precursor can be effectively prevented from volatilizing, so that the precursor can be fully cross-linked and cured in the protective layer, thereby improving the ceramic conversion rate of the precursor and the densification efficiency of the composite material. Figure 2 The interval in is shown.
[0046] (3) High temperature cracking process
[0047] The prepared tooling is loaded into a high-temperature furnace and subjected to high-temperature pyrolysis according to a certain high-temperature pyrolysis system to ultimately obtain a ceramic-based composite material.
[0048] In some embodiments, the UV curing process satisfies at least one of the following: UV irradiation is performed at 0.1 cm-10 cm from the surface of the composite material; the intensity of the UV light is 30-80 mW / cm 3 ; The irradiation time is 2-30min; the irradiation angle is -45°~+45°, and when the irradiation angle is 0°, it is vertical irradiation.
[0049] The cross-linking curing degree of the protective layer is different with different UV irradiation intensities. The higher the UV intensity, the higher the curing degree of the protective layer. In the temperature range of 200-300°C, the protective layer is close to a densified film. If the curing degree of the protective layer is low, in the temperature range of 200-300°C, the protective layer is a porous film. The present invention can control the curing degree of the protective layer by controlling the irradiation intensity or irradiation time of the protective layer. The specific corresponding relationship is as follows: Figure 2 .
[0050] In some embodiments, the thickness of the protective layer obtained by UV curing is 30-600 μm.
[0051] Different application environments require composite materials with different porosities. Aircraft insulation components often use porous ceramic-based composite materials, and heat-resistant structural components mostly use densified ceramic-based composite materials. According to the different densification requirements of ceramic-based composite materials, the volatilization rate of small molecules in the impregnated matrix can be controlled by adjusting the thickness of the protective layer, and then the densification degree of the composite material can be adjusted by adjusting the thickness of the protective layer. When the protective layer is 30-150μm, it is a porous structure at 200-300℃, and the volatilization amount of small molecules in part of the impregnated matrix is greater than 10%. When the thickness of the protective layer is greater than 150μm, the volatilization amount of the impregnated matrix is less than 5wt%. Finally, the densification degree of the composite material is adjusted by adjusting the thickness of the protective layer, and the porosity of the composite material varies from 5-30%. The number of spraying is controlled at 3-20 times according to demand. For details of the SEM image of the protective layer, see Figure 2 .
[0052] In some embodiments, the impregnation matrix includes at least one of organic precursor solutions such as polycarbosilane, polyborosilazane, and polysilazane.
[0053] In some embodiments, the fiber used in the fiber preform includes at least one of carbon fiber, silicon carbide fiber, aluminum-containing ceramic fiber, and other ceramic fibers containing refractory metals (Hf, Zr, Ti, etc.);
[0054] In some embodiments, the UV-curable resin includes at least one of a SiC ceramic precursor containing an acrylic group, a SiBCN ceramic precursor containing an acrylic group, an acrylic resin, or other resins containing acrylic monomers.
[0055] In some embodiments, the high temperature cracking system is mainly divided into two stages. In the first stage, the composite material is heated to 150-350°C at a heating rate of 2-15°C / min and kept warm for 1-4h. In the second stage, the composite material is heated to 800-1100°C at a heating rate of 5-10°C / min.
[0056] In some other embodiments provided by the present invention, the manufacturing process of the ceramic-based composite material may also include a thermal curing process. That is to say, the manufacturing steps of the ceramic-based composite material may include multiple process rounds, and the multiple process rounds include process round A and process round B. Process round A is an impregnation process-ultraviolet light curing process-high temperature cracking process, and process round B is an impregnation process-thermal curing process-high temperature cracking process. Process round B can be executed before process round A. In some embodiments, the number of executions of process round B can be 2 to 4 times. Process round A can be executed after all process rounds B are executed. The number of executions of process round A can be 1 to 4 times.
[0057] The following describes a manufacturing process of a ceramic-based composite material, which may include six rounds of composite processes, as follows.
[0058] The 1st to 3rd round of composite process:
[0059] (1) Impregnation process
[0060] The fiber preform is immersed in a soaking bucket filled with a ceramic precursor impregnation matrix solution and immersed at room temperature for 4 hours. After the soaking is completed, the preform is taken out of the soaking bucket and the excess impregnation matrix on the surface is scraped off.
[0061] (2) Thermal curing process
[0062] The impregnated composite material is placed in a metal tooling, placed in an oven and cured at 300-400°C for 2-4 hours. After the heat curing process is completed, the composite material is taken out of the oven and reloaded into the graphite tooling.
[0063] (3) High temperature cracking process
[0064] The prepared tooling is loaded into a high-temperature furnace and subjected to high-temperature pyrolysis according to a certain high-temperature pyrolysis system to ultimately obtain a ceramic-based composite material.
[0065] The first to third rounds of composite processes mainly adopt the "impregnation-thermal curing-high temperature cracking" process route. The main reason is that the density of the composite material is relatively low in the early stage. The weight gain rate of the composite material after the impregnation process is greater than 15%. During high temperature cracking, the small molecules of the precursor volatilize in a large amount, which will cause the protective layer made of the UV-cured precursor to crack. The protective effect is relatively limited. The thermal curing process can achieve the curing of the impregnated matrix. After the first three rounds of composite processes are completed, the density of the composite material is greater than 1.3g / cm 3 .
[0066] The 4th to 6th round of composite process:
[0067] (1) Impregnation process
[0068] The fiber preform is immersed in a soaking bucket filled with a ceramic precursor impregnation matrix solution and immersed at room temperature for 4 hours. After the soaking is completed, the preform is taken out of the soaking bucket and the excess impregnation matrix on the surface is scraped off.
[0069] (2) UV curing process
[0070] The prepared UV precursor solution is sprayed on the surface of the impregnated composite material, and then a certain intensity of UV light is irradiated on the surface of the composite material for a certain time according to a certain UV curing system, and finally the composite material is placed in a graphite tooling. The specific implementation of the UV curing process can be referred to above.
[0071] (3) High temperature cracking process
[0072] The prepared tooling is loaded into a high temperature furnace and subjected to high temperature pyrolysis according to a certain high temperature pyrolysis system, and finally a ceramic matrix composite material is obtained. The final porosity of the composite material is 8%. The composite material can be used, for example, for heat-resistant structural parts of aircraft.
[0073] The 4th to 6th rounds of composite process mainly adopt the process route of "impregnation-UV curing-high temperature cracking". Since the weight gain rate of the impregnated matrix in the last three rounds is less than 10%, the use of UV-curing precursor to manufacture the protective layer can effectively prevent the volatilization of small molecules of the precursor, so that it can be fully cross-linked and cured in the protective layer, thereby improving the precursor ceramic conversion rate and the densification efficiency of the composite material.
[0074] Example 1
[0075] Take a 200mm×200mm fiber preform, place it in the solid polycarbosilane toluene solution impregnation matrix, and soak it at room temperature for 4 hours. After the impregnation is completed, take out the composite material. Put the composite material into the graphite tooling and put it into the oven, heat it to 400℃ at a heating rate of 10℃ / min, keep it warm for 2 hours, take it out after natural cooling, re-load it into the graphite tooling, and raise the temperature to 1000℃ at a heating rate of 10℃ / min for high temperature treatment. Repeat this process 3 times.
[0076] The UV-curable SiC ceramic precursor was used as the spray slurry. The prepared slurry was sprayed on the surface of the composite material using a sprayer. The composite material was placed 1 cm away from the UV lamp. The intensity of the UV light was 40 mW / cm 3 , irradiate for 5 minutes, repeat spraying 3 times, after the protective layer is cured, finally place the composite material in a graphite tooling, load it into a high-temperature cracking furnace, raise the temperature to 180°C at a heating rate of 3°C / min and keep it warm for 2 hours, then raise the temperature to 1000°C at a heating rate of 10°C / min for high-temperature treatment. This process is only performed once, and the final porosity of the composite material is 28.2%. The composite material prepared in Example 1 can be used for thermal insulation components of aircraft, for example.
[0077] Example 2
[0078] Take a 200mm×200mm fiber preform, place it in the solid polycarbosilane toluene solution impregnation matrix, and soak it at room temperature for 4 hours. After the impregnation is completed, take out the composite material. Put the composite material into the graphite tooling and put it into the oven, heat it to 400℃ at a heating rate of 10℃ / min, keep it warm for 2 hours, take it out after natural cooling, re-load it into the graphite tooling, and raise the temperature to 1000℃ at a heating rate of 10℃ / min for high temperature treatment. Repeat this process 3 times.
[0079] The UV-curable SiC ceramic precursor was used as the spray slurry. The prepared slurry was sprayed on the surface of the composite material using a sprayer. The composite material was placed 5 cm under a UV lamp with an intensity of 80 mW / cm 3 , irradiate for 20 minutes, repeat spraying 10 times, after the protective layer is cured, finally place the composite material in a graphite tooling, load it into a high-temperature cracking furnace, raise the temperature to 180°C at a heating rate of 2°C / min and keep it warm for 2 hours, then raise the temperature to 1000°C at a heating rate of 5°C / min for high-temperature treatment, repeat this process twice, and the final porosity of the composite material is 15.3%. The composite material prepared in Example 2 can be used for thermal insulation components or heat-resistant structural components of aircraft, for example.
[0080] Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the claims of the present invention.
Claims
1. A method for photocuring of ceramic matrix composite materials, characterized in that: include: Impregnation process: the fiber preform is immersed in an immersion barrel filled with a ceramic precursor impregnation matrix solution. After the immersion is completed, the preform is taken out of the immersion barrel and the excess impregnation matrix on the surface is scraped off; UV curing process: spray the prepared UV precursor solution on the surface of the impregnated composite material, irradiate the composite material surface with UV light to form a protective layer on the composite material surface, and finally place the composite material in a graphite tooling; High temperature cracking process: The graphite tooling containing the composite material is loaded into a high temperature furnace and subjected to high temperature cracking according to the high temperature cracking system to finally obtain a ceramic-based composite material.
2. The method according to claim 1, characterized in that The UV curing process satisfies at least one of the following: UV irradiation is performed at 0.1 cm to 10 cm on the surface of the composite material; The intensity of UV light is 30-80mW / cm 3 ; The irradiation time is 2-30min; The irradiation angle is -45°~+45°; The number of times of spraying the UV precursor solution is controlled within 3-20 times; The thickness of the protective layer obtained by UV curing is 30-600 μm.
3. The method according to claim 2, characterized in that The ceramic matrix composite material finally obtained satisfies any of the following: Finally, the ceramic matrix composite material is used for thermal insulation components of aircraft, and the thickness of the protective layer is 30-150 μm; Finally, the ceramic matrix composite material is used for heat protection structural parts of aircraft, and the thickness of the protective layer is 150-600 μm.
4. The method according to claim 1, characterized in that: The impregnation matrix solution includes at least one of the following organic precursor solutions: polycarbosilane, polyborosilazane, and polysilazane.
5. The method according to claim 1, characterized in that The fibers used in the fiber preform include at least one of the following: carbon fibers, silicon carbide fibers, Al-containing ceramic fibers, Hf-containing ceramic fibers, Zr-containing ceramic fibers, and Ti-containing ceramic fibers.
6. The method according to claim 1, characterized in that The ultraviolet light precursor is a resin containing acrylic monomers.
7. The method according to claim 1, characterized in that The ultraviolet light precursor comprises at least one of the following: a SiC ceramic precursor containing an acrylic acid group, a SiBCN ceramic precursor containing an acrylic acid group, and an acrylic resin.
8. The method according to any one of claims 1 to 7, characterized in that The manufacturing steps of the ceramic matrix composite material include multiple process rounds, and the multiple process rounds include process round A and process round B. Process round A is an impregnation process-ultraviolet light curing process-high temperature cracking process, and process round B is an impregnation process-thermal curing process-high temperature cracking process; After process round B is fully executed, process round A is executed.
9. The method according to claim 8, characterized in that The method satisfies at least one of the following: Process run A was used at the stage where the weight gain of the impregnated substrate was <10%. The number of executions of process round B is 2 to 4 times; the number of executions of process round A is 1 to 4 times; After the process B is completed, the density of the composite material is greater than 1.3g / cm 3 ; After all the process rounds B are executed, the final porosity of the composite material is 5-30%; The heat curing process includes: placing the impregnated composite material into a metal tooling, placing it in an oven and curing it at 300-400°C for 2-4 hours, and after the heat curing process is completed, taking the composite material out of the oven and re-loading it into the graphite tooling; The high temperature cracking system includes two stages. In the first stage, the composite material is heated to 150-350°C at a heating rate of 2-15°C / min and kept warm for 1-4 hours. In the second stage, the composite material is heated to 800-1100°C at a heating rate of 5-10°C / min.
10. A ceramic matrix composite material, characterized in that: The ceramic-based composite material is prepared by the method according to any one of claims 1 to 9.
11. An aircraft, characterized in that: The aircraft comprises the ceramic-based composite material according to claim 10, and the ceramic-based composite material is applied to a heat insulation component or a heat protection structural component of the aircraft.
Citation Information
Patent Citations
Ceramic matrix composite material employing silicon alkyne-modified SiBCN as precursor and preparation method of ceramic matrix composite material
CN104591768A
Method for improving performance of ceramic-based composite material prepared by RMI process and prepared ceramic-based composite material
CN111848219A
Method for preparing ceramic-based composite material by interface-layer-free process
CN111892405A
High-density ceramic-based composite material and preparation method thereof
CN113979784A
Preparation method of novel ultraviolet curing prepreg
CN117510939A