Concrete exposed aggregate facing treating agent and use method thereof

By spraying an exposed aggregate finishing treatment agent composed of epoxy resin and other components on the surface of concrete components, and utilizing the synergistic effect of organic-inorganic composite retarder and hydration retarder, the problem of difficulty in achieving the exposed aggregate effect in the existing technology is solved. Significantly improve the decorative properties and yield of concrete.

CN118754716APending Publication Date: 2024-10-11CHONGQING GRAPHENE RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410780100.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult to achieve an exposed effect on cured concrete components with the existing technology, resulting in concrete color difference problems and insufficient decoration.

Method used

Provides a concrete exposed aggregate finishing treatment agent, including epoxy resin, water reducing agent, retardant, thickener, film-forming aid and defoaming agent, prepared by spraying on the inner surface of the mold and stirring at a specific temperature , form a suitable proportion and utilize the synergistic effect of organic-inorganic composite retarder and hydration retarder to extend the setting time of concrete and significantly improve the exposed effect.

Benefits of technology

It achieves no rapid solidification on the surface of concrete components, facilitates water gun flushing of laitance, significantly improves the exposed effect and decoration, and precisely controls the exposed depth by controlling the proportion of raw materials, prolongs the setting time, and improves the exposed effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete surface treatment, and particularly relates to a concrete exposed aggregate facing treatment agent and a use method. The concrete exposed aggregate veneer treating agent comprises epoxy resin, a water reducing agent, a retarder, a thickening agent, a coalescing agent and a defoaming agent. The concrete exposed aggregate facing treatment agent is sprayed to the inner surface of a mold, the outer surface of a solidified and formed concrete member cannot be rapidly solidified, laitance on the surface of the concrete member can be conveniently washed away through a water gun, in other words, internal aggregate can be exposed, the aggregate exposing effect is achieved, and by controlling mixing of the raw materials in different proportions, the concrete exposed aggregate facing treatment agent can be obtained. The bone exposing effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete surface treatment, and in particular relates to a concrete exposed aggregate finishing agent and a use method thereof. Background Art

[0002] Concrete, abbreviated as "concrete", refers to an engineering composite material that uses cementing materials to bind granular aggregates (usually called aggregates) into a whole. Generally speaking, concrete refers to cement as a cementing material, sand and stone as aggregates, and water (which may contain admixtures and additives) in a certain proportion, which is mixed and obtained by mixing. It is widely used in civil engineering.

[0003] During the concrete production and processing process, many problems are usually caused by the color difference of concrete. If the color difference problem cannot be solved, a large amount of concrete waste will be produced.

[0004] By making the concrete surface have an exposed effect, the color difference problem of concrete can be solved, and the decorativeness and yield rate of buildings and concrete parts can be significantly improved.

[0005] The existing method of producing the exposed effect of concrete is usually to react the surface of the concrete with a retarder, and then use a water gun to wash the slurry on the surface of the concrete after the reaction is completed, thereby exposing the internal aggregate of the concrete, that is, forming an exposed effect on the concrete surface. However, for concrete components that have been cured, the exposed effect cannot be achieved by using a retarder. Summary of the invention

[0006] In view of this, an object of the present invention is to provide a concrete exposed aggregate finishing agent and a method of use.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] In a first aspect, the present application provides a concrete exposed aggregate finishing agent, which comprises an epoxy resin, a water reducing agent, a retarder, a thickener, a film-forming aid, a defoaming agent and water.

[0009] Optionally, the epoxy resin is selected from bisphenol A epoxy resin.

[0010] Optionally, the water reducing agent comprises hydroxycarboxylic acid and / or hydroxycarboxylate and aminocarboxylic acid and / or aminocarboxylate.

[0011] Optionally, the mass ratio of the hydroxycarboxylic acid and / or hydroxycarboxylate to the aminocarboxylic acid and / or aminocarboxylate is 6-8:6-8.

[0012] Optionally, the retarder includes a hydration retarder and an organic-inorganic composite retarder.

[0013] Optionally, the hydration retarder is selected from polyols, polyol derivatives or a combination thereof.

[0014] Optionally, the mass ratio of the hydration retarder to the organic-inorganic composite retarder is 6-12:6-10.

[0015] Optionally, the organic-inorganic composite retarder comprises sodium hexametaphosphate, sodium pyrophosphate, sodium citrate and tartaric acid.

[0016] Optionally, the mass ratio of the sodium hexametaphosphate, sodium pyrophosphate, sodium citrate and tartaric acid is 5-15::3-7:2-5:4-8.

[0017] Optionally, the mass ratio of the sodium phosphate, aluminum hydroxide, sodium nitrite, calcium titanate, maleic anhydride, sucrose, calcium hexonate, cross-linking inhibitor and water is 15-25: 5-15: 2-8: 3-5: 4-6: 2-4: 4-6: 0.5-1.5: 45-70.

[0018] Optionally, the film-forming aid is selected from at least one of styrene acrylic emulsion, alkyl ketene dimer emulsion (AKD emulsion) and anionic surfactant.

[0019] Optionally, the defoaming agent is selected from at least one of a polyether defoaming agent, a silicone defoaming agent and an alcohol defoaming agent with a carbon number ≥10.

[0020] Optionally, the thickener is selected from hydroxypropyl methylcellulose ether.

[0021] Optionally, the concrete exposed aggregate finishing agent includes, by mass percentage: 10-15 parts of epoxy resin, 12-16 parts of water reducer, 12-22 parts of retarder, 1.5-2.5 parts of thickener, 2.5-43.5 parts of film-forming aid and 0.5-1.5 parts of defoamer.

[0022] Optionally, the preparation method of the concrete exposed aggregate finishing agent comprises the following steps:

[0023] The epoxy resin and the organic-inorganic composite retarder are mixed, heated to 45-55° C., stirred, and then the hydration retarder and the organic-inorganic composite retarder are added, and stirring is continued at a temperature of 45-55° C., and then a thickener, a film-forming aid, a defoamer and water are added, and stirred to obtain the concrete exposed aggregate finishing agent.

[0024] In a second aspect, the present application also provides a method for using the above-mentioned concrete exposed aggregate finishing agent, comprising the following steps:

[0025] The concrete exposed aggregate finishing agent is sprayed on the inner surface of the mold, and after solidification, concrete is added into the mold, and after solidification, the mold is demoulded.

[0026] The beneficial effects of the present invention include:

[0027] The present invention sprays the exposed aggregate finishing agent on the inner surface of the mold, so that the outer surface of the solidified concrete component does not solidify quickly, and the floating slurry on the surface can be washed clean with a water gun, that is, the internal aggregate is exposed, and the exposed effect is achieved. The exposed effect is improved by controlling the mixing of raw materials in different proportions.

[0028] The present invention has a better retarding effect on cement through the synergistic effect of the organic-inorganic composite retarder and the hydration retarder, and can also prolong the setting time of concrete, further improving and enhancing the exposure effect;

[0029] The present invention selects a specific hydration retarder (polyol, polyol derivative or a combination of the two), and can utilize the hydroxyl groups in the polyol and / or polyol derivative to be adsorbed on the surface of cement particles, and then form hydrogen bonds with oxygen atoms on the surface of the hydration product. At the same time, the hydroxyl groups can associate with water molecules through hydrogen bonds, so that a layer of stable solvated water film is formed on the surface of the cement particles, thereby inhibiting the hydration process of the cement. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the term "parts" in the present invention refers to parts by mass. It should also be understood that the following embodiments are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in the field according to the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only an example in a suitable range, that is, those skilled in the art can make a selection within a suitable range according to the description herein, and are not limited to the specific values ​​​​exemplified below.

[0031] Example 1

[0032] A concrete exposed aggregate finishing agent is prepared specifically according to the following steps:

[0033] S1. Mix 15 parts of sodium hexametaphosphate, 3 parts of sodium pyrophosphate, 5 parts of sodium citrate and 4 parts of tartaric acid to prepare an organic-inorganic composite retarder;

[0034] S2. Add 6 parts of hydroxycarboxylates and 8 parts of aminocarboxylates and / or aminocarboxylates to 10 parts of bisphenol A epoxy resin E-44, stir at 50°C for 5 minutes, then add 6 parts of propylene glycol and 6 parts of organic-inorganic composite retarder, continue stirring at 50°C, then add 2 parts of hydroxypropyl methylcellulose ether, 3 parts of styrene acrylic emulsion and 1 part of polyether defoamer THIX-288, continue stirring at 46°C for 5 minutes to prepare a concrete exposed aggregate finishing agent.

[0035] Example 2

[0036] A concrete exposed aggregate finishing agent is prepared specifically according to the following steps:

[0037] S1. Mix 5 parts of sodium hexametaphosphate, 7 parts of sodium pyrophosphate, 2 parts of sodium citrate and 8 parts of tartaric acid to prepare an organic-inorganic composite retarder;

[0038] S2. Add 7 parts of hydroxycarboxylate and 7 parts of aminocarboxylic acid and / or aminocarboxylate to 12 parts of bisphenol A epoxy resin E-42, stir at 50°C for 5 minutes, then add 9 parts of pentaerythritol and 8 parts of organic-inorganic composite retarder, continue stirring at 50°C, then add 2 parts of hydroxypropyl methylcellulose ether, 3 parts of AKD emulsion and 1 part of silicone defoamer

[0039] DE-1177, continue stirring at 50℃ for 5 minutes to obtain concrete exposed aggregate finishing agent.

[0040] Example 3

[0041] A concrete exposed aggregate finishing agent is prepared specifically according to the following steps:

[0042] S1. Mix 10 parts of sodium hexametaphosphate, 5 parts of sodium pyrophosphate, 3 parts of sodium citrate and 5 parts of tartaric acid to prepare an organic-inorganic composite retarder;

[0043] S2. Add 8 parts of hydroxycarboxylate and 8 parts of aminocarboxylic acid and / or aminocarboxylate to 15 parts of bisphenol A epoxy resin E-42, stir at 50°C for 5 minutes, then add 12 parts of pentaerythritol and 10 parts of organic-inorganic composite retarder, continue stirring at 50°C, then add 2 parts of hydroxypropyl methylcellulose ether, 3 parts of styrene acrylic emulsion and 1 part of polyether defoamer THIX-288, continue stirring at 52°C for 5 minutes to prepare a concrete exposed aggregate finishing agent.

[0044] Comparative Example 1

[0045] The difference between this comparative example and Example 1 is that it does not contain an organic-inorganic composite retarder.

[0046] Comparative Example 2

[0047] The difference between this comparative example and Example 1 is that glycerol is not contained.

[0048] Performance Testing

[0049] The exposed aggregate finishing agent of concrete prepared in Examples 1-3 and Comparative Examples 1-2 was sprayed on the inner surface of the mold respectively, and concrete was added into the mold after curing. The mold was demoulded after curing, and the initial setting time and the final setting time were recorded in the process; and the results were tested.

[0050] Exposed depth, usage is 30g / m 2 , the results are shown in Table 1.

[0051] Table 1 Test results

[0052] Group Initial setting time Final setting time Exposed Depth Example 1 15h 20h 3.3mm Example 2 16.5h 18h 2.6mm Example 3 15.5h 19h 2.7mm Comparative Example 1 7h 11h 1.1mm Comparative Example 2 6h 10h 1.4mm

[0053] As shown in Table 1, the initial setting time of Examples 1-3 is ≥15h, the final setting time is ≥18h, and the exposed depth is ≥2.6mm. The results show that the present invention can prevent the outer surface of the concrete component after solidification from being rapidly solidified by spraying the exposed aggregate finishing agent on the inner surface of the mold, so that the floating slurry on the surface can be washed clean with a water gun, that is, the internal aggregate will be exposed, and the exposed effect can be achieved, and the exposed effect can be improved by controlling the mixing of raw materials in different proportions, especially the exposed depth can be accurately controlled.

[0054] As shown in Table 1, compared with Comparative Examples 1 and 2, the initial setting time and resetting time of Example 1 are significantly prolonged, and the exposed depth is significantly increased. This result shows that the present invention has a better retarding effect on cement through the synergistic effect of the organic-inorganic composite retarder and the hydration retarder, and can also prolong the final setting time of concrete, thereby further improving the exposed effect.

[0055] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A concrete exposed aggregate finishing agent, characterized in that: The concrete exposed aggregate finishing agent comprises epoxy resin, water reducing agent, retarder, thickener, film-forming aid and defoamer.

2. The concrete exposed aggregate finishing agent according to claim 1, characterized in that: The epoxy resin is selected from bisphenol A epoxy resin.

3. The concrete exposed aggregate finishing agent according to claim 1, characterized in that: The water reducing agent includes hydroxycarboxylic acid and / or hydroxycarboxylate and aminocarboxylic acid and / or aminocarboxylate.

4. The concrete exposed aggregate finishing agent according to claim 3, characterized in that: The mass ratio of the hydroxycarboxylic acid and / or hydroxycarboxylate to the aminocarboxylic acid and / or aminocarboxylate is 6-8:6-8.

5. The concrete exposed aggregate finishing agent according to claim 1, characterized in that: The retarder includes a hydration retarder and an organic-inorganic composite retarder.

6. The concrete exposed aggregate finishing agent according to claim 5, characterized in that: The mass ratio of the hydration retarder to the organic-inorganic composite retarder is 6-12:6-10.

7. The concrete exposed aggregate finishing agent according to claim 5, characterized in that: The organic-inorganic composite retarder comprises sodium hexametaphosphate, sodium pyrophosphate, sodium citrate and tartaric acid.

8. The concrete exposed aggregate finishing agent according to claim 1, characterized in that: The film-forming aid is selected from at least one of styrene acrylic emulsion, alkyl ketene dimer emulsion and anionic surfactant.

9. The concrete exposed aggregate finishing agent according to claim 1, characterized in that: Calculated by weight, the concrete exposed aggregate finishing agent includes: 10-15 parts of epoxy resin, 12-16 parts of water reducer, 12-22 parts of retarder, 1.5-2.5 parts of thickener, 2.5-43.5 parts of film-forming aid and 0.5-1.5 parts of defoamer.

10. The method for using the concrete exposed aggregate finishing agent according to any one of claims 1 to 9, characterized in that: The following steps are involved: The concrete exposed aggregate finishing agent is sprayed on the inner surface of the mold, and after solidification, concrete is added into the mold, and after solidification, the mold is demoulded.