Method for preparing strontium titanate modification layer on zirconium oxide surface based on molten salt method, product and application

By using the molten salt method to prepare a strontium titanate modification layer on the surface of zirconia, and introducing elements such as strontium, calcium, and magnesium, the problem of insufficient bioactivity and osseointegration ability of zirconia ceramics is solved, and better bone formation and therapeutic effects are achieved. , expanding its application in the field of implants.

CN118754718AActive Publication Date: 2024-10-11HANGZHOU ERRAN TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410810170.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-11
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The biological activity and osseointegration ability of zirconia ceramics in the field of implants are insufficient, and the existing modification technology has limited effects and cannot effectively improve its clinical application.

Method used

A strontium titanate modified layer is prepared on the surface of zirconia using the molten salt method. By depositing the titanium dioxide layer and introducing elements such as strontium, calcium, and magnesium, a nanoparticle layer is formed to promote bone formation and osseointegration.

Benefits of technology

It improves the osseointegration ability of zirconia implants, enhances bone formation and bone repair processes, enhances biocompatibility and therapeutic effects, and expands the application of zirconia ceramics in the field of implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754718A_ABST
    Figure CN118754718A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a strontium titanate modification layer on a zirconium oxide surface based on a molten salt method, which comprises the following steps: (1) mixing titanium sulfate, urea and water to obtain a precursor liquid A, putting zirconium oxide ceramic into the precursor liquid A, heating to a boiling state, keeping for a period of time, taking out the zirconium oxide ceramic, and carrying out heat treatment A to obtain a strontium titanate modification layer; preparing a titanium dioxide film on the surface of zirconium oxide; (2) mixing an H2O2 aqueous solution, ammonia water and deionized water, adding metatitanic acid, stirring and dissolving to obtain a precursor liquid B, putting the zirconium oxide prepared with the titanium dioxide film into the precursor liquid B, standing and reacting for a period of time in a room temperature environment, and depositing to obtain zirconium oxide modified with a titanium dioxide precursor layer; and (3) mixing a molten salt medium, strontium salt and an organic solvent into slurry, coating the surface of the zirconium oxide modified with the titanium dioxide precursor layer with the slurry, and performing heat treatment B to prepare the strontium titanate modified layer on the surface of the zirconium oxide. The strontium titanate layer prepared on the zirconium oxide surface by the method disclosed by the invention can be tightly combined with a zirconium oxide substrate, and is non-toxic and non-corrosive to a human body; according to the method, high-content Sr, Mg and Ca elements can be introduced, strontium ions, calcium ions, magnesium ions and the like can be released for a long time at the implantation part, then bone formation is promoted, proliferation and differentiation of osteoblasts and formation of new bone tissues are promoted, and then the osseointegration capacity of the zirconium oxide implant is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface modification of zirconium oxide ceramics, and in particular to a method, product and application of preparing a strontium titanate modification layer on the surface of zirconium oxide based on a molten salt method. Background Art

[0002] Zirconia ceramics are used in the field of implants because of their corrosion resistance, stable chemical properties, good biocompatibility and superior mechanical properties. However, the biological inertness and weak bone integration ability of zirconia itself severely limit the application and promotion of its implant products in clinical practice. In order to improve the biological activity and bone integration ability of zirconia implants, sandblasting and acid etching techniques are often used in clinical practice to improve the surface roughness of zirconia, increase the coupling sites between the surface and bones, and the number of active functional groups. However, the former is prone to cause microcracks on the surface of zirconia, while the latter has extremely limited effect on the modification of chemically inert zirconia. In addition to sandblasting and acid etching, laser treatment, ion implantation, bionic deposition and biological modification are also used for surface modification of zirconia implants, but the modification effects of the above technologies are limited and cannot achieve the ideal modification effect.

[0003] Strontium plays an important role in human bone health. It is responsible for improving bone strength and protecting bone health. It is an essential element for the human body. In terms of bone defect treatment, strontium has a dual regulatory effect on bone regeneration and bone repair, namely: promoting osteoblast proliferation and differentiation, while inhibiting osteoclast proliferation and differentiation, ultimately promoting bone formation and inhibiting bone resorption. Compared with growth factors and other factors and drugs used for bone regeneration, strontium has the advantages of low cost, low risk and good stability. It is often used in clinical practice to treat osteoporosis (strontium ranelate) and modify artificial bone repair materials to improve bone-promoting ability. In addition to strontium, elements such as calcium, magnesium and zinc (calcium and magnesium are both elements of the same family as strontium) also have the ability to promote bone formation and bone regeneration.

[0004] Li et al. (Magnetron sputtering of strontium nanolayer on zirconia implant to enhance osteogenesis, Materials Science & Engineering C, 2021.5.19) disclosed a method of depositing a strontium nanolayer on a zirconia implant by magnetron sputtering to enhance osteogenesis. In this technical solution, a nano-strontium titanate coating is deposited on the surface of the zirconia implant by physical deposition, but the thickness of the prepared nano-strontium titanate coating is as high as 400 nm, while the Sr content in the coating is only 1.16±0.18 at%. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention discloses a method for constructing a strontium titanate modification layer on the surface of a zirconia implant. The strontium titanate layer prepared on the zirconia surface can be tightly combined with the zirconia substrate and is non-toxic and non-corrosive to the human body. The method can introduce high content of Sr, Mg, and Ca elements and can release strontium ions, calcium ions, magnesium ions, etc. at the implant site for a long time, thereby promoting bone formation, promoting the proliferation and differentiation of osteoblasts and the formation of new bone tissue, thereby improving the bone integration ability of the zirconia implant, and providing a new modification technology idea for the further application and development of zirconia in the implant field.

[0006] The specific technical solutions are as follows:

[0007] A method for preparing a strontium titanate modification layer on a zirconium oxide surface based on a molten salt method, comprising:

[0008] (1) titanium sulfate, urea and water are mixed to obtain a precursor liquid A, a zirconia ceramic is placed in the precursor liquid A, heated to a boiling state and maintained for a period of time, and then the zirconia ceramic is taken out, and after heat treatment A, a titanium dioxide film is prepared on the surface of the zirconia;

[0009] (2) mixing an aqueous H2O2 solution, an aqueous ammonia solution and deionized water, adding metatitanic acid and stirring to dissolve, to obtain a precursor liquid B, placing the zirconium oxide prepared with a titanium dioxide film in the precursor liquid B, and allowing the reaction to stand for a period of time at room temperature to deposit the zirconium oxide modified with a titanium dioxide precursor layer;

[0010] (3) mixing a molten salt medium, a strontium salt and an organic solvent into a slurry, coating the slurry on the surface of the zirconium oxide modified with the titanium dioxide precursor layer, and preparing a strontium titanate modified layer on the surface of the zirconium oxide after heat treatment B;

[0011] The molten salt medium is selected from sodium chloride, or a mixture of sodium chloride and potassium chloride;

[0012] The strontium salt is selected from a single strontium salt, or a mixed salt consisting of one or two of calcium salt and magnesium salt and strontium salt.

[0013] The invention first deposits two titanium dioxide layers on the surface of zirconia ceramics, gives the two titanium dioxide layers different morphological structures and reaction activities through different preparation processes, then constructs a strontium titanate modification layer on the surface of zirconia through a molten salt method, and regulates the components, morphology and structure of the in-situ generated strontium titanate modification layer through different types of introduced strontium salts and proportions of molten salt media, and finally prepares a strontium titanate layer containing osteogenic active elements such as calcium and magnesium and tightly combined with a substrate on the surface of zirconia; the strontium titanate layer prepared by the method has high contents of Sr, Mg and Ca, can release strontium ions, calcium ions and magnesium ions and the like at the affected part for a long time after being implanted into the human body to promote the formation of new bone tissue, and its bone integration ability is significantly improved.

[0014] The experiment found that if only one titanium dioxide layer was deposited, the amount of strontium titanate generated was too small, and the molten salt medium would corrode the zirconium oxide substrate; and if the source of the titanium dioxide precursor layer was changed, and metatitanic acid was replaced with tetrabutyl titanate, the titanium dioxide precursor layer could not be deposited;

[0015] In step (1):

[0016] The combination of titanium sulfate and urea can ensure that the precursor liquid A is stable at room temperature. Only when it decomposes under heating conditions will it slowly provide an alkaline atmosphere to combine with titanium ions to form a precipitate, thereby stably controlling the reaction process.

[0017] Preferred:

[0018] The molar ratio of titanium sulfate to urea is 1:(1 to 7), and more preferably 1:(3 to 7).

[0019] The concentration of titanium sulfate in the precursor liquid A is 0.1 to 1.0 mol / L, and more preferably 0.3 to 1.0 mol / L.

[0020] In step (1), the mixture is heated to a boiling state and maintained for 5 to 40 minutes to allow titanium to form a precipitate.

[0021] Preferably, the heat treatment A has a heat treatment temperature of 800 to 1000° C. and a holding time of 10 to 60 min;

[0022] More preferably, the heat treatment A has a heat treatment temperature of 850-950°C.

[0023] Titanic acid (H2TiO3) is insoluble in deionized water, but is soluble in a mixed solution of H2O2 / ammonia water. In step (2), when titanic acid is added to precursor liquid B, it is converted into an ammonium pertitanate solution and slowly degraded under room temperature to obtain a titanium dioxide precursor layer, i.e., a second titanium dioxide layer.

[0024] Preferred:

[0025] The molar ratio of the H2O2 aqueous solution to metatitanic acid is (3.7-5.2):1, based on the molar number of H2O2 in the H2O2 aqueous solution;

[0026] It has been found through experiments that if too much H2O2 is added in this step, the formation of the titanium dioxide precursor layer will be inhibited, resulting in too low a generation rate of strontium titanate, which in turn causes crack defects in the zirconium oxide matrix material, affecting the mechanical properties and durability.

[0027] Preferred:

[0028] The molar ratio of ammonia water to titanic acid is (2.0-2.4):1, based on the molar number of ammonium ions in ammonia water.

[0029] The concentration of metatitanic acid in the precursor solution B is 0.02 to 0.20 g / mL, and more preferably 0.07 to 0.12 g / mL.

[0030] In step (2), the reaction is allowed to stand at room temperature for 6 to 48 hours.

[0031] In step (3):

[0032] The strontium salt is selected from strontium carbonate, the calcium salt is selected from calcium carbonate, and the magnesium salt is selected from magnesium carbonate;

[0033] Experiments have found that the molten salt medium will provide liquid phase reaction conditions at high temperature. Titanium dioxide and carbonates are more likely to dissolve, dissociate, migrate and react in this liquid phase environment, and thus be better converted into strontium titanate. Tests have found that the amount and crystallinity of the strontium titanate modification layer prepared by the molten salt method are both high, indicating that this method is more conducive to improving the conversion rate and degree of crystal growth of the crystal.

[0034] The organic solvent is selected from one or more of methanol, ethanol and acetone; preferably, low-toxic ethanol.

[0035] Preferred:

[0036] The mass ratio of strontium salt to molten salt medium is (0.3-0.7):1; more preferably (0.5-0.6):1.

[0037] Preferably, the molten salt medium is selected from a mixture of sodium chloride and potassium chloride, and the mass ratio of sodium chloride to potassium chloride is (0.8-3.0):1; experiments have found that compared with sodium chloride alone as the molten salt medium, the strontium titanate nanoparticles in the strontium titanate modified layer prepared using the composite molten salt medium have higher morphology uniformity.

[0038] More preferably, the mass ratio of sodium chloride to potassium chloride is (0.8-1.2):1.

[0039] Preferably, in the heat treatment B, the heat treatment temperature is 800-1000° C., and the insulation time is 1-5 h; more preferably, the heat treatment temperature is 800-900° C., and the insulation time is 1-2 h.

[0040] The invention also discloses zirconium oxide with a strontium titanate modification layer on the surface, which is prepared according to the method.

[0041] The strontium titanate layer prepared by the present invention (the only alkaline earth metal element introduced is strontium) is a nanometer particle layer evenly distributed on the surface of zirconium oxide, with a layer thickness of about 150nm, wherein the particle size of the constituent unit nanometer particles is 10-100nm.

[0042] The strontium titanate layer (calcium and magnesium elements are introduced simultaneously) prepared by the present invention is a nanometer particle layer evenly distributed on the surface of zirconium oxide, and the layer thickness is about 150-250nm. Experiments have found that when strontium and calcium are introduced as elements, the strontium titanate layer is about 150nm thick and consists of large grains of 0.4 to 1.5μm. This is because the introduced calcium will enter the strontium titanate lattice in the form of solid solution, causing lattice distortion and abnormal crystal growth; when strontium and magnesium are introduced as elements, the strontium titanate layer is about 150nm thick and consists of irregular polyhedral particles with a size of 100 to 300nm, with a high surface roughness, which is also caused by the solid solution of magnesium in the strontium titanate crystals; when strontium, calcium and magnesium are introduced at the same time, the strontium titanate layer is about 200 to 400nm thick and consists of tetrahedral nanoparticles with a size of 150 to 400nm along the plane direction, and the strontium titanate component structure is affected by the solid solution of calcium and magnesium at the same time.

[0043] The invention also discloses the application of the zirconium oxide with the surface covered with a strontium titanate modification layer in the field of biological implant materials.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] The invention discloses a method for constructing a strontium titanate modification layer on the surface of a zirconia implant. A layer of strontium titanate nanoparticles is prepared on the surface of the zirconia by a molten salt method, and the components and morphological structure of the strontium titanate layer are regulated by regulating the proportion of a molten salt medium and the types of active osteogenic elements introduced. Finally, a strontium titanate layer that is tightly combined with a substrate, completely covers the substrate, has a uniform morphology and controllable components is prepared on the surface of the zirconia.

[0046] The strontium titanate modification layer prepared on the surface of zirconia of the present invention introduces a large amount of osteogenic active elements such as strontium, calcium and magnesium into the surface of zirconia. After implantation into the human body, the modification layer can continuously release strontium ions, calcium ions and magnesium ions into the bone defect to promote bone formation and bone repair process in the affected area, thereby improving the bone integration ability of the zirconia implant. Strontium titanate and calcium and magnesium elements are non-toxic and non-corrosive to the human body, have low safety risks, are relatively stable, are not easy to decompose and deform, and can exist in a complex human body environment for a long time. The introduction and modification thereof have been applied in other artificial bone repair materials such as titanium metal implants and the like, and the biocompatibility and osteogenic performance thereof have also been fully verified. In summary, the strontium titanate modification layer can promote bone formation and bone regeneration process in the affected area after the zirconia implant is implanted by introducing osteogenic active ions such as strontium ions, calcium ions and magnesium ions into the surface of the zirconia implant, thereby ultimately improving the bone integration ability, implantation success rate and treatment effect of the zirconia implant, thereby expanding the application of zirconia ceramics in the implant field. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a SEM image of the zirconium oxide with titanium dioxide film prepared in step 1) of Example 1;

[0048] Figure 2 This is a SEM image of the zirconium oxide modified with a titanium dioxide precursor layer prepared in step 2) of Example 1;

[0049] Figure 3 The XRD spectrum of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 1;

[0050] Figure 4 The cross-sectional SEM image, planar SEM image, EDS image and element relative content diagram of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 1;

[0051] Figure 5 This is a SEM image of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 6;

[0052] Figure 6 This is the XRD pattern of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 9;

[0053] Figure 7 The cross-sectional SEM image, planar SEM image, EDS image and element relative content diagram of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 9;

[0054] Figure 8 This is the XRD pattern of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 11;

[0055] Fig. 9 The cross-sectional SEM image, planar SEM image, EDS image and element relative content diagram of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 11;

[0056] Fig.10 This is the XRD pattern of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 13;

[0057] Fig.11 The cross-sectional SEM image, planar SEM image, EDS image and element relative content diagram of the strontium titanate modified layer on the surface of zirconium oxide prepared in Example 13;

[0058] Fig.12 The XRD spectrum and planar SEM image of the strontium titanate modified layer on the surface of zirconium oxide prepared in Comparative Example 1;

[0059] Fig.13 This is a planar SEM image of the strontium titanate modified layer on the surface of zirconium oxide prepared in Comparative Example 3;

[0060] Fig.14This is a planar SEM image of the strontium titanate modified layer on the surface of zirconium oxide prepared in Comparative Example 4. DETAILED DESCRIPTION

[0061] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.

[0062] Example 1

[0063] 1) Titanium sulfate and urea were dissolved in deionized water at a molar ratio of 1:3 to prepare a precursor solution A with a titanium sulfate concentration of 0.3 mol / L, zirconia ceramics were placed in the solution, heated to boiling state and kept for 15 minutes, then the zirconia ceramics were taken out and kept at 900°C for 30 minutes, and a titanium dioxide film was successfully prepared on the surface of the zirconia;

[0064] Figure 1 The SEM image of the zirconium oxide with titanium dioxide film prepared in this step shows that the titanium dioxide film is evenly covered and is composed of titanium dioxide particles with a particle size of 30 to 45 nm.

[0065] 2) Mix H2O2 aqueous solution (30wt%) and deionized water in a volume ratio of 1.5:1 to obtain 40mL of a mixed solution, add 9mL of concentrated ammonia water (25wt%) and stir until uniform, then add 3.4g of titanic acid (based on the molar number of H2O2 in the H2O2 aqueous solution, the molar ratio of the H2O2 aqueous solution to the titanic acid is 3.7:1; based on the molar number of ammonium ions in the ammonia water, the molar ratio of the ammonia water to the titanic acid is 2:1, the same below) and stir until dissolved to obtain a precursor solution B with a concentration of 0.07g / mL; place the zirconium oxide prepared with a titanium dioxide film therein, let it stand for reaction at room temperature for 12h, and deposit the zirconium oxide modified with a titanium dioxide precursor layer;

[0066] Figure 2 The SEM image of the zirconium oxide modified with the titanium dioxide precursor layer prepared in this step shows that the titanium dioxide precursor layer is composed of titanium dioxide particles with a particle size of less than 10 nm.

[0067] 3) Weigh 0.8 g of sodium chloride and 1.0 g of potassium chloride in a mass ratio of 0.8:1 and mix them to obtain 1.8 g of molten salt medium, then weigh 0.9 g of strontium carbonate in a mass ratio of strontium salt: molten salt medium of 0.5:1, mix them with the molten salt medium and grind them until there is no obvious granularity, and add a small amount of anhydrous ethanol to grind them into slurry; apply the slurry on the surface of zirconium oxide modified with a titanium dioxide precursor layer, and keep it at 850°C for 2 hours, and finally prepare a strontium titanate modified layer on the surface of zirconium oxide.

[0068] Figure 3(a) and (b) are XRD spectra of the sample prepared in this example in different diffraction angle ranges. It is found that the main phase of the sample is the base component zirconium oxide, and strontium titanate is also present. The main peak (110) of strontium titanate appears near 32.4°, which proves the formation of strontium titanate.

[0069] Figure 4 The cross-sectional SEM image, planar SEM image, corresponding EDS image and element relative content diagram of the sample prepared in this embodiment show that the strontium titanate modification layer of the sample is about 150nm thick, is aggregated from 30-50nm nanoparticles, and has a relatively smooth surface. The EDS image shows that the sample surface contains elements such as strontium, further confirming the presence of strontium titanate. The element relative content diagram specifically shows that the relative content of strontium in the strontium titanate modification layer of the sample is 9.88at% (unless otherwise specified, the relative content of elements in the present invention refers to the atomic content).

[0070] Example 2

[0071] The preparation process is basically the same as that in Example 1, except that in step 2):

[0072] The volume ratio of the H2O2 aqueous solution and deionized water was replaced with 2:1, and the volume of the mixed solution was still 40 mL. At this time, the molar ratio of the H2O2 aqueous solution to titanic acid was 4.4:1.

[0073] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 1.

[0074] Example 3

[0075] The preparation process is basically the same as that in Example 1, except that in step 2):

[0076] The amount of titanic acid added was replaced with 4.8 g to obtain a precursor solution with a concentration of 0.12 g / mL. At this time, the molar ratio of the H2O2 aqueous solution to the titanic acid was 5.2:1.

[0077] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 1.

[0078] Example 4

[0079] The preparation process is basically the same as that in Example 1, except that in step 3):

[0080] 0.9 g of sodium chloride and 0.9 g of potassium chloride were weighed and mixed in a mass ratio of 1:1 to obtain 1.8 g of molten salt medium.

[0081] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 1.

[0082] Example 5

[0083] The preparation process is basically the same as that in Example 1, except that in step 3):

[0084] 0.98 g of sodium chloride and 0.82 g of potassium chloride were weighed and mixed in a mass ratio of 1.2:1 to obtain 1.8 g of molten salt medium.

[0085] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 1.

[0086] Example 6

[0087] The preparation process is basically the same as that in Example 1, except that in step 3):

[0088] 1.35 g of sodium chloride and 0.45 g of potassium chloride were weighed and mixed in a mass ratio of 3:1 to obtain 1.8 g of molten salt medium.

[0089] Figure 5 This is a planar SEM image of the sample prepared in this example. It is observed that the sample is composed of nanoparticles with a particle size of 10 to 100 nm and has slightly poor morphology uniformity.

[0090] Example 7

[0091] The preparation process is basically the same as that in Example 1, except that in step 3):

[0092] 1.8 g of sodium chloride was added as the molten salt medium, and no potassium chloride was added.

[0093] SEM characterization showed that the morphology of the strontium titanate layer prepared in this example was similar to that in Example 6.

[0094] Example 8

[0095] The preparation process is basically the same as that in Example 1, except that in step 3):

[0096] The mass of strontium carbonate is replaced with 1.08 g, and the mass ratio of strontium salt to molten salt medium is 0.6:1.

[0097] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 1.

[0098] Example 9

[0099] The preparation process is basically the same as that in Example 1, except that in step 3):

[0100] 0.9 g of strontium carbonate was replaced with a mixed salt consisting of 0.45 g of strontium carbonate and 0.45 g of calcium carbonate.

[0101] Figure 6 (a) and (b) are XRD spectra of the sample prepared in this embodiment within different diffraction angle ranges, respectively. It is found that the main phase of the sample is the base component zirconium oxide, and strontium titanate is also present. The main peak (110) of strontium titanate appears near 33.0°, which proves the formation of strontium titanate and explains that the solid solution doping of calcium ions causes lattice distortion of strontium titanate, causing the diffraction peak to shift toward a larger angle.

[0102] Figure 7 The cross-sectional SEM image, planar SEM image, corresponding EDS image and element relative content diagram of the sample prepared in this embodiment show that the strontium titanate modification layer of the sample is about 150nm thick, and is composed of large grains of 0.4 to 1.5μm along the planar direction, with a high surface roughness. The EDS image shows that the sample surface contains elements such as strontium and calcium, further confirming the presence of strontium titanate and the strontium titanate lattice distortion caused by the solid solution of calcium ions. The element relative content diagram specifically shows that in the strontium titanate modification layer, the relative content of strontium is 3.18%, and the relative content of calcium is 9.78%.

[0103] Example 10

[0104] The preparation process is basically the same as that in Example 9, except that in step 3):

[0105] The masses of strontium carbonate and calcium carbonate are each replaced with 0.54 g, and the total mass of the strontium salt is 1.08 g. At this time, the mass ratio of the strontium salt to the molten salt medium is 0.6:1.

[0106] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Example 9.

[0107] Embodiment 11

[0108] The preparation process is basically the same as that in Example 1, except that in step 3):

[0109] 0.9 g of strontium carbonate was replaced with a mixed salt consisting of 0.45 g of strontium carbonate and 0.45 g of magnesium carbonate.

[0110] Figure 8(a) and (b) are the XRD spectra of the sample prepared in this embodiment within different diffraction angle ranges, respectively. It is observed that the main phase of the sample is the base component zirconium oxide, and strontium titanate is also present. The main peak (110) plane of strontium titanate appears on the left side of 32.4°, which proves the formation of strontium titanate and explains that the solid solution doping of magnesium ions causes lattice distortion of strontium titanate, causing the diffraction peak to shift to a smaller angle direction.

[0111] Fig. 9 The cross-sectional SEM image, planar SEM image, corresponding EDS image and element relative content diagram of the sample prepared in this embodiment show that the strontium titanate modification layer of the sample is about 150nm thick and is formed by paving irregular polyhedral nano-grains of 100 to 300nm, so that the surface roughness of the modification layer is relatively high. The EDS image shows that the surface of the sample contains elements such as strontium and magnesium, which further confirms the presence of strontium titanate and the strontium titanate lattice distortion caused by the solid solution of magnesium ions. The element relative content diagram specifically shows that in the strontium titanate modification layer, the relative content of strontium is 5.38%, and the relative content of magnesium is 1.05%.

[0112] Example 12

[0113] The preparation process is basically the same as that in Example 11, except that in step 3):

[0114] The masses of strontium carbonate and magnesium carbonate are both replaced with 0.54 g, and the total mass of strontium salt is 1.08 g. At this time, the mass ratio of strontium salt to molten salt medium is 0.6:1.

[0115] XRD and SEM characterizations showed that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example were basically the same as those in Example 11.

[0116] Embodiment 13

[0117] The preparation process is basically the same as that in Example 1, except that in step 3):

[0118] 0.9 g of strontium carbonate was replaced with a mixed salt consisting of 0.3 g of strontium carbonate, 0.3 g of calcium carbonate and 0.3 g of magnesium carbonate.

[0119] Fig.10 (a) and (b) are XRD spectra of the sample prepared in this embodiment within different diffraction angle ranges, respectively. It is found that the main phase of the sample is the base component zirconium oxide, and strontium titanate is also present. The main peak (110) of strontium titanate appears near 32.5°, which proves the formation of strontium titanate and explains that the simultaneous solid solution doping of calcium and magnesium elements causes lattice distortion of strontium titanate and shifts the diffraction peak to a larger angle.

[0120] Fig.11The cross-sectional SEM image, planar SEM image, corresponding EDS image and element relative content diagram of the sample prepared in this embodiment show that the strontium titanate modification layer of the sample has a thickness of about 200 to 400 nm, is composed of 150 to 400 nm tetrahedral nano-grains along the plane direction, and has a high surface roughness. The EDS image shows that the sample surface contains elements such as strontium, calcium and magnesium, further confirming the presence of strontium titanate and the strontium titanate lattice distortion caused by the co-solution of calcium ions and magnesium ions. The element relative content diagram specifically shows that in the strontium titanate modification layer, the relative content of strontium is 0.95%, the relative content of calcium is 7.09%, and the relative content of magnesium is 1.11%.

[0121] Embodiment 14

[0122] The preparation process is basically the same as that in Example 13, except that in step 3):

[0123] The masses of strontium carbonate, calcium carbonate and magnesium carbonate are all replaced with 0.36 g, and the total mass of strontium salt is 1.08 g. At this time, the mass ratio of strontium salt to molten salt medium is 0.6:1.

[0124] XRD and SEM characterizations showed that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example were basically the same as those in Example 13.

[0125] Comparative Example 1

[0126] 1) Titanium sulfate and urea were dissolved in deionized water at a molar ratio of 1:3 to prepare a precursor solution A with a titanium sulfate concentration of 0.3 mol / L, zirconia ceramics were placed in the solution, heated to boiling state and kept for 15 minutes, then the zirconia ceramics were taken out and kept at 900°C for 30 minutes, and a titanium dioxide film was successfully prepared on the surface of the zirconia;

[0127] 2) 0.8 g of sodium chloride and 1.0 g of potassium chloride were weighed and mixed in a mass ratio of 0.8:1 to obtain 1.8 g of molten salt medium, and then 0.9 g of strontium carbonate was weighed in a mass ratio of strontium salt: molten salt medium of 0.5:1, mixed with the molten salt medium and ground until there was no obvious granularity, and a small amount of anhydrous ethanol was added to grind into slurry; the slurry was coated on the surface of zirconium oxide modified with titanium dioxide film, and kept at 850°C for 2 hours, and finally a strontium titanate modified layer was prepared on the surface of zirconium oxide.

[0128] Fig.12From the XRD spectrum and planar SEM images of the samples prepared for this comparative example, it was observed that although strontium titanate appeared in the physical phase of the sample, large cracks and defects appeared on the surface of its modified layer, and the zirconia substrate was corroded by the molten salt, and large particles were pulverized into small particles, which easily led to crack defects in the zirconia matrix material and affected the mechanical properties and durability. This may be because the titanium dioxide precursor layer was not deposited, resulting in a relatively excessive amount of molten salt, which then invaded the surface of the zirconia substrate.

[0129] Comparative Example 2

[0130] Step (1) is exactly the same as in Example 1;

[0131] (2) Dissolve 1 mL of tetrabutyl titanate in 4 mL of anhydrous ethanol to prepare an ethanol solution of tetrabutyl titanate, and apply the solution to the surface of the zirconia ceramic treated in step (1), let it stand for 2 hours, and wait for the tetrabutyl titanate to react with water vapor in the air to hydrolyze to generate titanium dioxide.

[0132] Step (3) is exactly the same as in Example 1.

[0133] XRD and SEM characterizations show that the phase composition and morphology of the zirconium oxide modified with a strontium titanate layer prepared in this example are substantially the same as those in Comparative Example 1, which may be because the amount of titanium dioxide precursor deposited by the hydrolysis of tetrabutyl titanate is too small.

[0134] Comparative Example 3

[0135] The preparation process is basically the same as that in Example 1, except that in step 2):

[0136] The ratio of H2O2 solution and deionized water was changed to 3:1, and the volume of the mixed solution was still 40 mL. At this time, the molar ratio of H2O2 aqueous solution to titanic acid was 7.8:1.

[0137] Fig.13 From the planar SEM image of the sample prepared for this comparative example, it was observed that the morphology of the sample was similar to that of comparative example 1. The zirconium oxide particles were also corroded by the molten salt and pulverized into small particles, which was not conducive to the stability and durability of the zirconium oxide substrate. This may be because the excessive amount of hydrogen peroxide inhibited the deposition of the titanium dioxide precursor, resulting in a decrease in the amount of titanium dioxide deposition.

[0138] Comparative Example 4

[0139] The preparation process is basically the same as that in Example 1, except that in step 3):

[0140] 0.45 g of sodium chloride and 1.35 g of potassium chloride were weighed and mixed in a mass ratio of 1:3 to obtain 1.8 g of molten salt medium.

[0141] Fig.14 The plane SEM picture of the sample prepared in this comparative example shows that the strontium titanate modification layer of the sample is composed of 10-30nm nanoparticles, accompanied by obvious inter-particle sintering, and some large particle crystals with a size of about 200-300nm appear. The surface morphology is uneven and there are vacancy defects, which is not conducive to practical application.

[0142] Comparative Example 5

[0143] The preparation process is basically the same as that in Example 1, except that in step 3):

[0144] 1.8 g of potassium chloride was added as the molten salt medium, and no sodium chloride was added.

[0145] The SEM characterization showed that the morphology of the strontium titanate layer prepared in this comparative example was similar to that in comparative example 4.

[0146] The above-mentioned embodiments are preferred embodiments, but the protection scope of the present invention is not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above-mentioned embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.

Claims

1. A method for preparing a strontium titanate modification layer on the surface of zirconium oxide based on a molten salt method, It is characterized in that include: (1) titanium sulfate, urea and water are mixed to obtain a precursor liquid A, a zirconia ceramic is placed in the precursor liquid A, heated to a boiling state and maintained for a period of time, and then the zirconia ceramic is taken out, and after heat treatment A, a titanium dioxide film is prepared on the surface of the zirconia; (2) H 2 O 2 The aqueous solution, ammonia water and deionized water are mixed, and metatitanic acid is added and stirred to dissolve to obtain a precursor liquid B, and the zirconium oxide prepared with a titanium dioxide film is placed in the precursor liquid B, and allowed to react for a period of time at room temperature to deposit the zirconium oxide modified with a titanium dioxide precursor layer; (3) mixing a molten salt medium, a strontium salt and an organic solvent into a slurry, coating the slurry on the surface of the zirconium oxide modified with the titanium dioxide precursor layer, and preparing a strontium titanate modified layer on the surface of the zirconium oxide after heat treatment B; The molten salt medium is selected from sodium chloride, or a mixture of sodium chloride and potassium chloride; The strontium salt is selected from a single strontium salt, or a mixed salt consisting of one or two of calcium salt and magnesium salt and strontium salt.

2. The method for preparing a strontium titanate modification layer on the surface of zirconium oxide based on a molten salt method according to claim 1, It is characterized in that In step (1): The molar ratio of titanium sulfate to urea is 1:(1-7); The concentration of titanium sulfate in the precursor liquid A is 0.1-1.0 mol / L.

3. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to claim 1, It is characterized in that In step (1): Heat to boiling and keep for 5 to 40 minutes; The heat treatment A has a heat treatment temperature of 800 to 1000° C. and a heat preservation time of 10 to 60 minutes.

4. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to claim 1, It is characterized in that In step (2): H 2 O 2 H in aqueous solution 2 O 2 The number of moles, H 2 O 2 The molar ratio of the aqueous solution to titanic acid is (3.7-5.2):1; The molar ratio of ammonia water to titanic acid is (2.0-2.4):1, based on the molar number of ammonium ions in ammonia water. The concentration of titanic acid in the precursor liquid B is 0.02 to 0.20 g / mL.

5. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to claim 1, It is characterized in that In step (2), the reaction is allowed to stand at room temperature for 6 to 48 hours.

6. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to claim 1, It is characterized in that In step (3): The strontium salt is selected from strontium carbonate, the calcium salt is selected from calcium carbonate, and the magnesium salt is selected from magnesium carbonate; The organic solvent is selected from one or more of methanol, ethanol and acetone; The mass ratio of strontium salt to molten salt medium is (0.3-0.7):1; The heat treatment B has a heat treatment temperature of 800-1000° C. and a heat preservation time of 1-5 hours.

7. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to claim 1, It is characterized in that In step (3): The molten salt medium is selected from a mixture of sodium chloride and potassium chloride, and the mass ratio of sodium chloride to potassium chloride is (0.8-3.0):

1.

8. The method for preparing a strontium titanate modified layer on the surface of zirconium oxide based on an impregnation-heat treatment method according to any one of claims 1 to 7, Features: In step (1): The molar ratio of titanium sulfate to urea is 1:(3-7); The concentration of titanium sulfate in the precursor liquid A is 0.3-1.0 mol / L; The heat treatment A has a heat treatment temperature of 850-950°C and a heat preservation time of 10-60 minutes; In step (2): The concentration of metatitanic acid in the precursor liquid B is 0.07 to 0.12 g / mL; In step (3): The mass ratio of strontium salt to molten salt medium is (0.5-0.6): 1 The mass ratio of sodium chloride to potassium chloride in the molten salt medium is (0.8-1.2):1; The heat treatment B has a heat treatment temperature of 800-900° C. and a heat preservation time of 1-2 hours.

9. Zirconium oxide with a surface-covered strontium titanate modification layer prepared according to the method of any one of claims 1 to 8.

10. Use of the zirconium oxide with a strontium titanate modification layer on its surface according to claim 9 in the field of biological implant materials.

Citation Information

Patent Citations

  • Method for preparing titanium-containing catalyst carrier

    CN101733083A

  • Preparation method of strontium titanate nano powder

    CN104192892A

  • Method for preparing SrTiO3 powder by means of molten salt method

    CN106554035A

  • Method for preparing aluminum oxide micro-nano structure layer on zirconium oxide surface based on secondary precipitation-heat treatment as well as product and application thereof

    CN116751077A

  • Preparation method, product and application of zirconia surface micro-nano structure based on precipitation-heat treatment