Corrosion inhibitor for acidizing and fracturing of oil field as well as preparation method and application of corrosion inhibitor
A cationic surfactant is prepared through the Borch reductive amination and dimethyl sulfate quaternization reaction of pyridine-2,5-dicarboxaldehyde and aza-18-crown ether-6 under sodium borocyanide conditions. Used for acidification and fracturing in oil fields, it solves the problems of flammability, volatility and high toxicity of existing corrosion inhibitors, and achieves efficient metal corrosion protection and safe and environmentally friendly construction results.
Patent Information
- Application Number
- CN202410822074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-11
AI Technical Summary
The corrosion inhibitors in existing acidified fracturing fluids contain flammable and volatile ethanol and highly toxic propargyl alcohol, which results in greater construction safety and environmental impact, and it is difficult to control the corrosion rate to meet industry standards.
Using sodium borocyanide as the reducing agent, pyridine-2,5-dicarboxaldehyde and aza-18-crown ether-6 were used to perform Borch reductive amination reaction in a weak acid environment, and under weak alkaline conditions with Dimethyl sulfate undergoes a quaternization reaction to form a cationic surfactant that is used to form a protective layer to prevent metal corrosion.
It achieves good dispersion and corrosion inhibition performance in acid liquid, reduces the corrosion rate, improves construction safety and environmental benefits, and has a simple synthesis method, making it suitable for oilfield acid fracturing applications.
Smart Images

Figure BDA0004909362090000041 
Figure BDA0004909362090000051 
Figure BDA0004909362090000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petroleum extraction, and in particular relates to a corrosion inhibitor for oilfield acid fracturing and a preparation method and application thereof. Background Art
[0002] Acid fracturing of oil wells is one of the main measures for stabilizing and increasing production in various oil fields in my country. The principle is to inject acid fracturing fluid into the formation through the oil well pipe string, and the acid fracturing fluid reacts with the limestone and other components in the formation to generate soluble substances. At the same time, under the action of high pressure, the pores of the formation are enlarged. When the soluble substances are discharged from the formation with the acid, the permeability of the oil-producing layer is increased, thereby achieving the purpose of increasing production.
[0003] However, during the construction process, the corrosion of metal by acid will not only damage the ground equipment and downhole pipelines, but also the large amount of corroded iron ions will form iron oxide precipitation under certain conditions, affecting the acidizing effect, and sometimes may cause sudden rupture of downhole pipes, causing serious economic losses. Therefore, adding corrosion inhibitors to the acidizing fracturing fluid is a necessary anti-corrosion measure.
[0004] The corrosion inhibitor can be adsorbed on the surface of the metal pipe to form a continuous protective film, which prevents the acid from contacting the metal and reacting, thus playing a protective role. This protective film can prevent the hydrogen ions in the acid or other corrosive media from directly contacting the metal surface, reducing the corrosion reaction rate.
[0005] During the acid fracturing process, the surface of the metal pipe column will first react with the acid solution, and the metal ions produced after the reaction will complex with the corrosion inhibitor in the fracturing fluid to form an insoluble complex. This complex can cover the surface of the metal pipe column, isolating the acid solution and the metal pipe column, preventing further reaction, thereby reducing the corrosion effect.
[0006] CN104109529A discloses an acidizing corrosion inhibitor and a preparation method thereof, wherein the acidizing corrosion inhibitor is mainly made of the following raw materials in parts by weight: 39-41 parts of acetophenone, 24-26 parts of formaldehyde, 9-11 parts of ethylenediamine, 24-25 parts of anhydrous ethanol, 1-2 parts of concentrated hydrochloric acid, and 1-3 parts of propargyl alcohol. The acidizing corrosion inhibitor of the invention uses acetophenone, formaldehyde, anhydrous ethanol, concentrated hydrochloric acid, ethylenediamine and propargyl alcohol as raw materials. Through reasonable compounding, the obtained acidizing corrosion inhibitor has good dispersibility in acid solution, and can achieve good compatibility with acid solution and other acidizing additives without adding other synergists and surfactants; has good corrosion inhibition performance, reaches the first-level industry standard, and does no harm to the core during the acidizing process; has little impact on the human body and the environment, and has a small amount used during on-site construction, which not only reduces the cost of acidizing construction, but also improves the safety of on-site construction, has good economic and environmental benefits, and is suitable for promotion and application. However, this product contains a large amount of ethanol, which is flammable and volatile, and its vapor can form an explosive mixture with air. It also contains propargyl alcohol, which is highly toxic and volatile. Summary of the invention
[0007] The present invention aims at the above-mentioned deficiencies of the prior art and provides a corrosion inhibitor for oilfield acid fracturing and a preparation method thereof. The corrosion inhibitor of the present invention has the characteristics of simple synthesis method and good corrosion inhibition effect.
[0008] According to the first aspect of the present invention, the present invention discloses a method for preparing a corrosion inhibitor for oilfield acid fracturing, the preparation method comprising: in the presence of sodium borocyanide as a reducing agent, pyridine-2,5-dicarboxaldehyde and aza-18-crown ether-6 undergo Borch reduction amination reaction in a weakly acidic environment; secondly, in the presence of weakly alkaline conditions, the reduction amination reaction product undergoes a quaternization reaction with dimethyl sulfate in acetone under reflux.
[0009] In the present invention, preferably, based on 1 mole of pyridine-2,5-dicarboxaldehyde, the aza-18-crown-6 and dimethyl sulfate are 1.6-2.4 moles and 2.7-3.6 moles, respectively; more preferably, based on 1 mole of pyridine-2,5-dicarboxaldehyde, the aza-18-crown-6 and dimethyl sulfate are 1.8-2.2 moles and 3.3-3.6 moles, respectively.
[0010] In the present invention, preferably, the mass ratio of sodium borocyanide to pyridine-2,5-dicarbaldehyde is 1-1.5:1.
[0011] In the present invention, preferably, the weakly acidic environment is pH 3-4.
[0012] In the present invention, preferably, the reductive amination reaction temperature is 50-60° C. and the time is 4-6 h.
[0013] In the present invention, preferably, the weakly alkaline environment is pH 8-9.
[0014] In the present invention, preferably, the mass ratio of acetone to pyridine-2,5-dicarbaldehyde is 20-30:1.
[0015] In the present invention, preferably, the quaternization reaction time is 6-12 hours.
[0016] According to a more specific preferred embodiment, the method for preparing the corrosion inhibitor for oilfield acid fracturing comprises the following steps:
[0017] (1) adding pyridine-2,5-dicarboxaldehyde, aza-18-crown-6, deionized water, and sodium borocyanide into a reactor, adjusting the pH to 3-4 with sulfuric acid, and heating and keeping the reaction;
[0018] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.5-1h, allowed to stand for 0.5-1h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0019] (3) dissolving the distillation residue with acetone, adjusting the pH to 8-9 with potassium carbonate solution, adding dimethyl sulfate dropwise, maintaining the pH to 8-9 with potassium carbonate solution during the reaction, and heating to reflux after the addition of dimethyl sulfate is completed;
[0020] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0021] In the present invention, preferably, the mass ratio of the deionized water to pyridine-2,5-dicarbaldehyde is 15-20:1.
[0022] The synthetic reaction equation of the main product of the corrosion inhibitor for oilfield acid fracturing of the present invention is as follows:
[0023]
[0024] According to a second aspect of the present invention, the present invention discloses a corrosion inhibitor for oilfield acid fracturing, wherein the molecular structure of the main product of the corrosion inhibitor is as follows:
[0025]
[0026] In a third aspect, the present invention discloses the application of the above corrosion inhibitor in oil field acid fracturing.
[0027] The corrosion inhibitor for oilfield acid fracturing of the present invention is a cationic surfactant. The three quaternary ammonium functional groups can adsorb the molecule to the metal surface to form a protective layer. The molecule contains multiple nitrogen and oxygen elements, which can provide lone pairs of electrons to the metal surface to reduce corrosion. The crown ether can protect the metal ions in the ring center to prevent further corrosion. Methyl sulfate has a hydrophobic effect and can form a hydrophobic barrier on the metal surface, so that the corrosive liquid cannot approach the metal, thereby further strengthening the corrosion inhibition. The synthesis method of the corrosion inhibitor for oilfield acid fracturing of the present invention is easy to master, and the corrosion inhibition effect is good. The corrosion rate in 20wt% hydrochloric acid can be controlled at 1g / (m 2 h). DETAILED DESCRIPTION
[0028] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0029] The technical solution of the invention is further described below in conjunction with specific embodiments:
[0030] Example 1
[0031] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.064 mol of aza-18-crown ether-6, 81 g of deionized water, and 5.4 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 50°C, and keep the reaction warm for 4 hours;
[0032] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.5 h, allowed to stand for 0.5 h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0033] (3) Dissolve the distillation residue with 108 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.108 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 6 h;
[0034] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0035] Example 2
[0036] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.096 mol of aza-18-crown ether-6, 108 g of deionized water, and 8.1 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 60°C, and keep the reaction warm for 4 hours;
[0037] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 1 hour, allowed to stand for 1 hour, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0038] (3) Dissolve the distillation residue with 162 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.112 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 12 h;
[0039] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0040] Example 3
[0041] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.068 mol of aza-18-crown ether-6, 92 g of deionized water, and 6.6 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 55°C, and keep the reaction warm for 5 hours;
[0042] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.6 h, allowed to stand for 0.8 h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0043] (3) Dissolve the distillation residue with 111 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.12 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 8 h;
[0044] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0045] Example 4
[0046] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.092 mol of aza-18-crown ether-6, 104 g of deionized water, and 7.3 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 52°C, and keep the reaction warm for 6 hours;
[0047] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.5 h, allowed to stand for 0.7 h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0048] (3) Dissolve the distillation residue with 154 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.126 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 8 h;
[0049] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0050] Example 5
[0051] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.072 mol of aza-18-crown-6, 89 g of deionized water, and 7.2 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 50°C, and keep the reaction warm for 6 hours;
[0052] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.9 h, allowed to stand for 0.7 h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0053] (3) Dissolve the distillation residue with 128 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.134 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 10 h;
[0054] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0055] Example 6
[0056] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.088 mol of aza-18-crown ether-6, 92 g of deionized water, and 7.6 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 60°C, and keep the reaction warm for 5.5 hours;
[0057] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 1 hour, allowed to stand for 1 hour, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0058] (3) Dissolve the distillation residue with 133 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.144 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 8 h;
[0059] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0060] Example 7
[0061] (1) Add 0.04 mol of pyridine-2,5-dicarboxaldehyde, 0.08 mol of aza-18-crown ether-6, 95 g of deionized water, and 7.5 g of sodium borocyanide into a reactor, adjust the pH to 3-4 with sulfuric acid, heat to 58°C, and keep the reaction warm for 4.5 hours;
[0062] (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.9 h, allowed to stand for 0.6 h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure;
[0063] (3) Dissolve the distillation residue with 150 g of acetone, adjust the pH to 8-9 with potassium carbonate solution, add 0.128 mol of dimethyl sulfate dropwise, and maintain the pH at 8-9 with potassium carbonate solution during the reaction. After the addition of dimethyl sulfate is complete, heat and reflux for 8 h;
[0064] (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
[0065] Example 8 Corrosion Rate Test
[0066] The static corrosion rate of the corrosion inhibitor of the present invention (Examples 1-7) at normal pressure was determined with reference to SY / T 5405-2019 "Performance Test Method and Evaluation Method of Corrosion Inhibitor for Acidification", the test conditions are shown in Table 1, and the test results are shown in Table 2. At the same time, the AN-Y001 corrosion inhibitor of Hebei Annuo Environmental Protection Technology Co., Ltd. was used for comparative experiments.
[0067] Table 1 Test conditions
[0068]
[0069] Table 2 Corrosion rate test results, g / (m 2 h)
[0070] Test samples Method 1 Method 2 Method 3 Method 4 Example 1 0.87 0.91 0.88 1.1 Example 2 0.85 0.87 0.84 1.05 Example 3 0.88 0.89 0.87 1.1 Example 4 0.84 0.86 0.84 1.01 Example 5 0.85 0.88 0.85 1.02 Example 6 0.83 0.86 0.83 0.99 Example 7 0.8 0.85 0.84 0.99 AN-Y001 4.21 5.12 4.54 6.8
[0071] From Table 1 we can see that:
[0072] (1) The corrosion rate of the oilfield acid fracturing corrosion inhibitor (Examples 1-7) of the present invention in 20wt% hydrochloric acid at a concentration of 0.5wt% at 60°C is 0.90g / (m 2 ·h) below, the minimum is 0.80g / (m 2 ·h), while the corrosion rate of the comparative experiment is 4.21g / (m 2 h), which is significantly higher than that of the present invention;
[0073] (2) The corrosion rate of the oilfield acid fracturing corrosion inhibitor (Examples 1-7) of the present invention in 20wt% hydrochloric acid at a concentration of 1.0wt% at 90°C is 1.0g / (m 2 ·h) below, the lowest is 0.85g / (m 2 ·h), while the corrosion rate of the comparative experiment is 5.12g / (m 2 h), which is significantly higher than that of the present invention;
[0074] (3) The corrosion rate of the oilfield acid fracturing corrosion inhibitor (Examples 1-7) of the present invention in 12wt% hydrochloric acid + 3wt% hydrofluoric acid at a concentration of 0.5wt% at 60°C is 0.90g / (m 2 ·h) below, the lowest is 0.83g / (m 2 ·h), while the corrosion rate of the comparative experiment is 4.54g / (m 2 h), which is significantly higher than that of the present invention;
[0075] (4) The corrosion rate of the oilfield acid fracturing corrosion inhibitor (Examples 1-7) of the present invention in 12wt% hydrochloric acid + 3wt% hydrofluoric acid at a concentration of 1.0wt% at 90°C is 1.2g / (m 2 ·h) below, the lowest is 0.99g / (m 2 ·h), while the corrosion rate of the comparative experiment is 6.8g / (m 2 h), which is significantly higher than that of the present invention.
[0076] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a corrosion inhibitor for oilfield acid fracturing, characterized in that: The preparation method comprises: in the presence of sodium borocyanide as a reducing agent, pyridine-2,5-dicarboxaldehyde and aza-18-crown ether-6 undergo Borch reduction amination reaction in a weak acid environment; secondly, in a weak alkaline condition, the reduction amination reaction product undergoes a quaternization reaction with dimethyl sulfate in a reflux state in acetone; Based on 1 mole of pyridine-2,5-dicarboxaldehyde, the aza-18-crown-6 and dimethyl sulfate are 1.6-2.4 moles and 2.7-3.6 moles, respectively; The reductive amination reaction temperature is 50-60°C and the time is 4-6h; The quaternization reaction time is 6-12h.
2. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: Based on 1 mole of pyridine-2,5-dicarboxaldehyde, the amounts of aza-18-crown-6 and dimethyl sulfate are 1.8-2.2 moles and 3.3-3.6 moles, respectively.
3. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: The mass ratio of the sodium borocyanide to pyridine-2,5-dicarbaldehyde is 1-1.5:
1.
4. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: The weakly acidic environment has a pH of 3-4.
5. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: The weakly alkaline environment is pH 8-9.
6. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: The mass ratio of acetone to pyridine-2,5-dicarbaldehyde is 20-30:
1.
7. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 1, characterized in that: The preparation method specifically comprises the following steps: (1) adding pyridine-2,5-dicarboxaldehyde, aza-18-crown-6, deionized water, and sodium borocyanide into a reactor, adjusting the pH to 3-4 with sulfuric acid, and heating and keeping the reaction; (2) The mixed solution was adjusted to pH <1 with sulfuric acid, stirred for 0.5-1h, allowed to stand for 0.5-1h, the remaining sodium borocyanide was quenched, the pH was adjusted to 6-7 with sodium hydroxide solution, extracted with chloroform, separated, and the chloroform phase was distilled to dryness under reduced pressure; (3) dissolving the distillation residue with acetone, adjusting the pH to 8-9 with potassium carbonate solution, adding dimethyl sulfate dropwise, maintaining the pH to 8-9 with potassium carbonate solution during the reaction, and heating to reflux after the addition of dimethyl sulfate is completed; (4) The reflux liquid was distilled to dryness under reduced pressure, and recrystallized with cyclohexane to obtain a light yellow solid, which was dried in an oven at 80° C. overnight to obtain a corrosion inhibitor product.
8. The method for preparing a corrosion inhibitor for oilfield acid fracturing according to claim 7, characterized in that: The mass ratio of the deionized water to pyridine-2,5-dicarboxaldehyde is 15-20:
1.
9. The corrosion inhibitor prepared according to any preparation method of claims 1-8.
10. Use of the corrosion inhibitor according to claim 9 in oil field acid fracturing.
Citation Information
Cited By
High-temperature acidizing corrosion inhibitor as well as preparation method and application thereof
CN119504634A