Novel aliphatic polycarbonate material as well as preparation method and application thereof
By using the combined use of epoxy haloalkanes and epoxy cyclohexane and bimetallic cobalt catalysts with quaternary ammonium groups in aliphatic polycarbonate materials, the problem of insufficient thermal and mechanical properties of existing materials has been solved and achieved More efficient performance improvements and simplified preparation processes.
Patent Information
- Application Number
- CN202410750621.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-30
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing aliphatic polycarbonate materials have deficiencies in thermal performance, strength and gas barrier, and existing modification methods are complex and have limited effects, making it difficult to significantly improve their performance while maintaining the material's superior properties.
Epoxy haloalkanes and epoxy cyclohexane are used as epoxy monomers, and the thermal stability of the material is improved by embedding carbonate haloester chain segments in the structure and using a bimetallic cobalt catalyst with a quaternary ammonium group for polymerization. , temperature tolerance and mechanical properties.
The thermal stability, temperature tolerance and mechanical properties of the material are significantly improved, its application scenarios are expanded, and the preparation process is simplified. The catalyst is easy to recycle and the reaction is simple and efficient.
Smart Images

Figure HDA0004887789020000011 
Figure HDA0004887789020000012 
Figure HDA0004887789020000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material chemistry, and in particular relates to a novel aliphatic polycarbonate material and a preparation method and application thereof. Background Art
[0002] Aliphatic polycarbonate materials are a type of material that is directly prepared using greenhouse gas carbon dioxide as raw material. This type of material is one of the effective ways to fix and utilize carbon dioxide and has good development prospects. The first aliphatic polycarbonate developed was polypropylene carbonate (PPC), a biodegradable material synthesized using carbon dioxide and propylene oxide as raw materials. The prepared material has a molecular weight between 20,000 and 100,000 and has good flexibility and biodegradability. However, since the main chain of the PPC molecule is an open-chain isopropyl structure, the molecule is flexible, resulting in a low glass transition temperature (T g ) is less than 40°C, and thermal decomposition separation is usually below 220°C, which has imposed certain restrictions on its promotion and application.
[0003] In order to improve the temperature application window of aliphatic polycarbonates, people use cyclohexane with a rigid six-membered ring structure to replace propylene oxide for alternating copolymerization to prepare new aliphatic polycarbonates, and continue to conduct in-depth research. Patents CN201711037217.X and CN 201711037215.0 use carbon dioxide and cyclohexane as monomer raw materials, and use organic zinc complexes as catalysts to prepare polycyclohexyl carbonate (PCHC) with a molecular weight of more than 20,000. Compared with traditional PPC, the glass transition temperature of PCHC polyester can reach above 110°C, and the thermal decomposition temperature can reach above 280°C, which greatly broadens the temperature application window of aliphatic polycarbonates. However, this material has certain defects in mechanical properties. Due to the presence of a six-membered alicyclic structure in the polyester main chain, the molecular structure is rigid but not tough enough. It is a hard and brittle material at room temperature with poor impact resistance. In view of this situation, many researchers use physical blending methods to improve the mechanical properties of PCHC. Patent CN202011040246.3 adds nano-silicon dioxide, lamellar wollastonite nanomaterials, glass fiber and other auxiliary ingredients, and obtains an organic-inorganic composite material through melt blending, which can improve the tensile strength of PCHC to a certain extent, but the preparation process of the material is relatively complicated. Patent [CN 202211016329.8] adds polyolefin elastomer POE and related additives, and modifies through melt blending, which can improve the elongation at break of PCHC to a certain extent, but POE has poor compatibility with PCHC, and phase separation is likely to occur if the formula is unreasonable or the operation is improper.
[0004] Physical modification operations are complicated and the degree of performance improvement is limited. In contrast, chemical modification methods are performed at the molecular level, and the effect is usually more significant. Patent CN 202111307477.0 uses methacryloyl chloride and its oxide as modification reagents to end-cap low molecular weight PCHC, reduce its terminal hydroxyl content, weaken the intermolecular hydrogen-chlorine reaction, thereby reducing crystallinity and increasing material toughness. Li Xiang and others from Northeast Normal University copolymerized lactide as the third component to obtain a terpolymer, but due to the large difference in properties between lactide and cyclohexene oxide and different activation methods, a binary or even ternary catalyst system is required, the catalysis is complex and the structural regulation of the chain segments is more difficult.
[0005] Therefore, how to maintain the advantageous properties of polycarbonate polymers while using a simple and efficient method to improve the comprehensive properties of polycarbonate materials such as thermal properties, strength and gas barrier properties, and promote the development of related products is a technical problem that technicians in this field urgently need to solve. Summary of the invention
[0006] In order to solve the problems existing in the prior art, one of the objectives of the present invention is to provide a new type of aliphatic polycarbonate material with relatively better thermal stability, temperature tolerance and mechanical properties.
[0007] The second object of the present invention is to provide a method for preparing a novel aliphatic polycarbonate material, which uses an independently synthesized catalyst to improve reaction efficiency, the catalyst is easy to recycle, and the polymerization reaction is simple and efficient.
[0008] The third object of the present invention is to provide a novel aliphatic polycarbonate material for use in the preparation of degradable products.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0010] A new type of aliphatic polycarbonate material is polymerized by carbon dioxide, cyclohexene oxide and epoxy halogenated alkane monomers under the action of a catalyst.
[0011] Optionally, the molar ratio of the epoxy cyclohexane to the epoxy halogenated alkane monomer is 1:0.5-2.0.
[0012] Preferably, in a specific embodiment of the present invention, the epoxyhaloalkane monomer is epichlorohydrin.
[0013] Optionally, the total molar amount of cyclohexene oxide and epichlorohydrin is used as the epoxy monomer dosage; the molar ratio of carbon dioxide to epoxy monomer is 0.5 to 1.5:1.
[0014] Optionally, the number average molecular weight of the material is 14,000 to 30,000.
[0015] Preferably, the material has a general structure as shown in formula (V): Among them, m:n=0.5~2.0:1.
[0016] The present invention uses epoxy halogenated alkanes and epoxy cyclohexane as epoxy monomers. Compared with the traditional PCHC introduced chemical modification, compared with the existing chemical modification methods, the invention creatively uses epoxy halogenated alkanes and embeds halogenated carbonate segments in the structure to improve the thermal stability, temperature tolerance and mechanical properties of the material, overcome the defects of existing similar materials, and expand the application scenarios of the material. At the same time, it also provides a better reaction site for further performance improvement and functional derivation of the ternary polyester, which has more development prospects.
[0017] Preferably, in a specific embodiment of the present invention, the catalyst is a bimetallic cobalt catalyst with a quaternary ammonium group; preferably, the catalyst has a general structure shown in formula (VI): Where X is a coordinated anion group;
[0018] Preferably, X is selected from 2,4-dinitrophenolate oxide anion, 3,5-bis(trifluoromethyl)phenolate oxide anion or trichloroacetate ion.
[0019] The total molar amount of cyclohexene oxide and epichlorohydrin is taken as the amount of epoxy monomer; the molar ratio of the catalyst to the epoxy monomer is 1:2000-4000.
[0020] The present invention adopts a novel bimetallic cobalt catalyst with quaternary ammonium group as polymerization catalyst, and its structural feature is that it has electrophilic-nucleophilic bifunctional property, and has two catalytic active centers, can well realize bimetallic coordinated catalytic process, therefore has higher catalytic activity, can be used alone, makes catalytic system simple and easy to recycle and reuse, and its structural feature is that two mononuclear cobalt structures are connected by biphenyl hard connection, so that the distance of catalytic active center is kept relatively fixed. The central metal is Co (III) cation, and its acidity is moderate, which can ensure that the monomer has good affinity, and after the reaction is finished, the polyester chain can also be relatively easily dissociated from the Co (III) of the active center, realize good chain transfer, and be conducive to the narrow distribution of polyester molecular weight. The quaternary ammonium group is a tetra-n-butylammonium structure, which has larger steric hindrance, and the electric force between it and its counter ion is weak, so that the counter ion has a stronger nucleophilic effect. The axially coordinated ions are all negative ion groups with strong electron-withdrawing ability, such as 2,4-dinitrophenoloxy anion, 3,5-bis(trifluoromethylphenoloxy) anion and trichloroacetate ion, which can stabilize the cobalt atom in the Co(III) oxidation state and maintain a high electrophilic ability.
[0021] The preparation method of the novel fatty carbonate material comprises dissolving and mixing epoxycyclohexane, epoxyhaloalkane and a catalyst under nitrogen protection, injecting carbon dioxide, stirring and heating, and separating and purifying after the reaction is completed to obtain the novel fatty carbonate material.
[0022] Preferably, in a specific embodiment of the present invention, the charging of carbon dioxide specifically includes first charging carbon dioxide to 80% of the set pressure, stirring and heating to the reaction temperature, and then additionally charging carbon dioxide to 100% of the set pressure;
[0023] The method also includes timing the reaction to control the reaction conversion rate to 50%, stopping the reaction, cooling to room temperature, releasing the remaining carbon dioxide and separating and purifying the reaction product;
[0024] Preferably, the separation and purification includes distilling off the unreacted alkylene oxide under reduced pressure to recover the raw materials, adding dichloromethane and 1M hydrochloric acid to the residual liquid after cooling, slowly stirring until it is evenly dissolved, adding methanol under stirring to precipitate, aging, filtering, and obtaining a pale yellow crude product, then dissolving the crude product with dichloromethane, precipitating with methanol again, repeating the process 2 to 3 times, washing, and drying, and the process is completed;
[0025] Preferably, the reaction pressure is 2.0-4.0 MPa; the reaction temperature is 25-45°C;
[0026] Preferably, the method further comprises first preparing the above-mentioned bimetallic cobalt catalyst with quaternary ammonium groups. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 1H-NMR spectrum of the intermediate compound I in the process of synthesizing the catalyst;
[0029] Figure 2 1H-NMR spectrum of the intermediate compound II in the process of synthesizing the catalyst;
[0030] Figure 3 1H-NMR spectrum of the intermediate compound III in the process of synthesizing the catalyst;
[0031] Figure 4 1H-NMR spectrum of the refined product prepared in Example 1;
[0032] Figure 5 The GPC chromatogram of the refined product prepared in Example 1;
[0033] Figure 6 The molecular weight fitting result of the refined product prepared in Example 1;
[0034] Figure 7 The thermogravimetric curve of the refined product prepared in Example 1;
[0035] Figure 8 The differential thermogravimetric curve of the refined product prepared in Example 1;
[0036] Fig. 9 This is the differential scanning calorimetry diagram of the purified product prepared in Example 1. DETAILED DESCRIPTION
[0037] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0038] The raw materials used in the following examples are all commercially available products, among which cyclohexene oxide was purchased from Shenma Nylon Chemical Co., Ltd. and epichlorohydrin was purchased from Sinopharm Chemical Reagent Co., Ltd. All of them were analytically pure, fully dried over calcium hydride, distilled, and sealed and stored for later use.
[0039] The catalyst used in the following examples has the general structure shown in formula (VI): Wherein X is a coordinated anion group; wherein X is selected from 2,4-dinitrophenoloxy anion, 3,5-bis(trifluoromethyl)phenoloxy anion or trichloroacetate ion.
[0040] The synthesis reaction process is shown in formula (VII):
[0041]
[0042] The specific synthesis process is:
[0043] (1) Preparation of Compound I
[0044] Place a 100ml round-bottom flask equipped with a magnetic rod in a low-temperature cooling liquid and start stirring. The temperature is controlled below 0°C. Dissolve 3,3'-diformyl-4,4'-biphenyl (24g, 0.1mol), cyclohexanediamine hydrochloride and the condensation product of salicylaldehyde (48.5g, 0.2mol) in 300ml of refined dichloromethane, add triethylamine (55ml, 0.4mmol), and add an appropriate amount of 5A molecular sieves. After reacting at room temperature for 24h, filter the solution, wash the filter cake with dichloromethane (50ml×5), collect the filtrate and distill under reduced pressure to obtain a crude product. Purify by column chromatography (dry loading; silica gel column; developing solvent: petroleum ether / ethyl acetate = 10 / 1) to obtain compound I in the form of a golden powder. Its 1H-NMR characterization results are as follows: Figure 1 As shown, the yield is 55.02 g, and the yield is about 85.6%.
[0045] (2) Preparation of Compound II
[0046] Take the refined compound I (32.14g, 0.05mol), add 200mL of dichloromethane, then add 14.41g (0.11mol) of anhydrous AlCl3, stir at room temperature to dissolve it; then add 50mL of dichloromethane solution containing 14.10g of chlorobutyryl chloride, and absorb the escaping HCl tail gas with dilute alkali solution. After the addition is completed, continue the reaction for 2.5 hours and then end the reaction. Add 100mL of ice water mixture to the reaction solution and stir vigorously to decompose the complex, then transfer to a separating funnel, let stand and separate, and wash the separated organic liquid phase with deionized water, 5% NaOH solution, and then wash with water until neutral. Evaporation concentration, cooling and crystallization, obtain the crude acylated intermediate, which is refined by dichloromethane to obtain 34.30g of pure product with a yield of about 80.0%.
[0047] The above acylated product was dissolved in 200 mL of anhydrous ethanol and 8.0 g of palladium carbon catalyst, and hydrogen was introduced. The reaction was allowed to react for 24 hours at room temperature of 25 degrees, and then the reaction was terminated. The reaction solution was concentrated to 1 / 2 volume by rotary evaporation, cooled naturally, and a white solid was precipitated. The solid was filtered, washed with alcohol, and dried to obtain 28.24 g of compound II. The 1H-NMR characterization results are as follows: Figure 2 As shown, the yield is about 85.1%.
[0048] (3) Preparation of Compound III
[0049] Add compound II (16.59 g, 0.02 mol), tri-n-butylamine 9.28 g (0.05 mol), a little KI and anhydrous ethanol 150 mL to the reactor, stir, heat and reflux for 24 hours, then stop the reaction. Concentrate under reduced pressure, cool and crystallize to precipitate a light yellow solid. Heat and dissolve the crude product again with an appropriate amount of anhydrous ethanol, cool to room temperature naturally, crystallize, filter and dry to obtain 21.95 g of quaternary ammonium compound, with a yield of about 92.5%.
[0050] Under nitrogen protection, the quaternary ammonium compound was dissolved in 100 mL of anhydrous dichloromethane. Under stirring conditions, 100 mL of a methanol solution containing 7.08 g of cobalt acetate was slowly added to continuously precipitate a red precipitate. After the addition was completed, the reaction was stopped after continuing to stir for 1 hour. The mixture was allowed to stand for aging for 0.5 hours to allow the precipitation to be complete. The filter cake was washed with an appropriate amount of methanol for 3 times and dried in vacuo to obtain a brick-red solid powder compound III, the 1H-NMR characterization results of which are shown as follows: Figure 3 As shown, the yield is 22.83 g,
[0051] Yield: 94.9%.
[0052] (4) Preparation of Compounds IVa-c
[0053] 0.01mol of compound III and 0.03mol of anhydrous LiCl were added to the reactor, and then 80mL of anhydrous dichloromethane was added and stirred to dissolve. The O2 introduction rate was adjusted, and the oxygen was turned off after bubbling oxidation at room temperature until it turned dark green. The organic phase was washed with saturated NaHCO3 solution and water respectively until neutral, and the desiccant was filtered out after adding anhydrous Na2SO4 to dry. Then 0.042mol of AgBF4 was added to react for 12 hours in the dark, and the insoluble matter was filtered out. Then 0.05mmol of sodium 2,4-dinitrophenolate or sodium 3,5-bistrifluoromethylphenolate or sodium trichloroacetate was added) and the reaction was continued to stir vigorously for 24 hours. The material was taken out, the inorganic salt was filtered out, and the filtrate was washed with saturated NaHCO3 solution and deionized water to neutrality, concentrated and crystallized to obtain dark green or black solid powder IVa~c, with yields of 88.9%, 85.2% and 81.4%, respectively, and dried and stored for use.
[0054] Example 1
[0055] This embodiment provides a synthesis process of a novel aliphatic polycarbonate material, and its synthesis process route is shown in the following formula (VIII):
[0056]
[0057] (VIII), the specific synthesis process is as follows:
[0058] (1) preparing an epoxy mixture: weighing cyclohexene oxide and halogenated epoxy propane in a molar ratio and mixing them uniformly;
[0059] (2) weighing a certain amount of dry catalyst into a flask in a dry nitrogen atmosphere, and then adding the epoxy mixture prepared in step (1) at a molar ratio of epoxy mixture: catalyst = 2000:1, stirring to dissolve;
[0060] (3) After the reactor is vacuum dried in advance, it is filled with low-pressure nitrogen for protection. Then, the material of step (2) is transferred to the reactor with a syringe and sealed. The reactor is placed in a heating jacket and then filled with carbon dioxide at 0.8 times the set pressure. Stirring is started and the temperature is raised. When the temperature reaches the set temperature, carbon dioxide is added to the set pressure and timing is started. The reaction is stopped when the reaction conversion rate reaches about 50% (inferred from the pressure gauge, this is to avoid the reaction system from solidifying due to deep reaction). The temperature is cooled to room temperature. After the remaining carbon dioxide is slowly released, the reactor is opened and a small amount of liquid is first drawn with a syringe for reaction process analysis. The remaining material is then separated and purified later.
[0061] (4) The material is drawn out and placed in a flask, and the unreacted alkylene oxide is first evaporated under reduced pressure to recover the raw material. After cooling, an appropriate amount of dichloromethane and a few drops of 1M hydrochloric acid are added to the residual liquid, and slowly stirred until it is evenly dissolved. Then, it is added to excess methanol under stirring for precipitation, aging, and filtering to obtain a light yellow crude product. The crude product is then dissolved with a small amount of dichloromethane, and precipitated with methanol again. This process is repeated 2 to 3 times, and washed and dried to obtain a refined white CO2 / CHO / ECH terpolymer product, which is the novel aliphatic polycarbonate material.
[0062] The epoxy monomer material ratio, catalyst dosage, reaction time, temperature and reaction product analysis results set in the process of synthesizing the novel aliphatic polycarbonate material provided by each embodiment of the present invention are shown in Table 1 below:
[0063] Table 1
[0064]
[0065] Note: n(epoxide): n(catalyst) = 2000, carbon dioxide pressure 3.0 MPa; TOF: catalyst conversion frequency
[0066] Comparative Example 1
[0067] This comparative example provides a fatty polycarbonate material, which is different from Example 1 in that the epichlorohydrin monomer ECH is omitted, and the CO2 / CHO binary polymer is prepared by polymerization using the same method as Example 1.
[0068] Comparative Example 2
[0069] This comparative example provides a fatty carbonate material, which is different from Example 1 in that propylene oxide is used instead of epichlorohydrin, and the CO2 / CHO / PPO terpolymer is prepared by polymerization using the same method as Example 1.
[0070] Comparative Example 3
[0071] This comparative example provides an aliphatic polycarbonate material, which is different from Example 1 in that the cyclohexene oxide monomer CHO is omitted, and the CO2 / ECH binary polymer is prepared by polymerization using the same method as Example 1.
[0072] Test example
[0073] 1. Performance characterization and comparison:
[0074] (1) Structural characterization: The product obtained in Example 1 of the present invention was 1 H NMR, molecular weight size and distribution analysis:
[0075] Take the product prepared in Example 1 and detect its hydrogen nuclear magnetic resonance spectrum as shown in Figure 4 As shown in the figure, the multiple peaks between the chemical shifts of 1.19 and 2.16 are the four methylene peaks on the cyclohexyl group, the peak at 3.72 is the chloromethyl peak, the peak at 4.38 is the peak of two methines in the ring, the peak at 4.51 is the methylene peak connected to the carbonic acid part in the ECH segment, and the peak at 5.12 chemical shift is the methine peak in the ECH segment. This shows that the sample is a ternary polyester structure. At the same time, there are very small peaks at the chemical shift of 3.2-3.6. These peaks are very small polyether structure peaks in the main chain, indicating that the main chain is basically an alternating copolymerized polyester structure, and the chemical structure selectivity of the reaction is good.
[0076] The molecular weight and distribution were determined by high temperature gel chromatography, with anhydrous tetrahydrofuran as the mobile phase, a flow rate of 1.00 ml / min, and polystyrene as the standard sample (for determining the molecular weight of polyester).
[0077] like Figure 5 The GPC chromatogram of the product of Example 1 shows that the peak time of the prepared CO2 / CHO / ECH terpolymer sample reaches 2 minutes, which is relatively wide. Figure 6 As shown in the figure, after molecular weight fitting, the number average molecular weight of the sample is 21.3kg / mol, the weight average molecular weight is 34.6kg / mol, and the molecular weight polydispersity distribution coefficient PDI value is about 1.62. The reason is that compared with binary polyester, there are three components in the ternary polyester reaction system, and the disorder of the reaction and the random termination factors encountered in the chain growth process are also increased, which leads to an increase in the difference in the size of the molecular chain. Therefore, the PDI is larger than the distribution coefficient of about 1.2 to 1.3 in binary copolymerization.
[0078] (2) Performance comparison:
[0079] ① Thermal stability: such as Figure 7The thermogravimetric graph of the product of Example 1 shows that the mass of the sample slowly decreases in the early stage. The reason is that a small amount of volatile solvent remains in the sample preparation process. It begins to decompose at 294°C and reaches the maximum weight loss rate at around 300°C. The decomposition temperature of the sample is concentrated in a narrow temperature range, indicating that the texture of the terpolymer is relatively uniform. This conclusion can also be drawn from Figure 8 As verified in the differential weight loss diagram shown, the sample exhibits a sharp thermal decomposition peak at 299°C.
[0080] Compared with the thermal decomposition peak temperature of about 280°C of the CO2 / CHO / PPO ternary polymer provided in Comparative Example 2, it is increased by nearly 20°C, indicating that after the third monomer is changed to epichlorohydrin, the thermal stability of the obtained polymer is improved to a certain extent.
[0081] ②DSC detects the changes in the aggregation state of the sample during the heating process. Fig. 9 It can be seen that the glass transition temperature of the product of Example 1 of the present invention is about 68.2°C, which is significantly higher than the glass transition temperature of 42°C of the CO2 / ECH copolymer with the same molecular weight provided in Comparative Example 3. This is because the CHO monomer introduces a rigid six-membered ring structure into the polyester main chain, which increases the rigidity of the chain and reduces the flexibility of the molecular chain, thereby enhancing the interaction force between molecules and making it difficult for the molecules to slide against each other, thereby significantly increasing the glass transition temperature.
[0082] For random copolymerized terpolymers, the glass transition temperature can be detected. The glass transition temperature is an important performance indicator of structural materials, which reflects the temperature tolerance of the material. The polypropylene carbonate products (PPC) currently in mass production have a glass transition temperature of only about 40°C, which is relatively low for structural materials, and to a certain extent limits the promotion of their application fields. Therefore, for this type of new material, having a higher glass transition temperature is an important indicator requirement, and the new material provided by the present invention has a positive significance for expanding the temperature use window of the material.
[0083] ③ Mechanical properties:
[0084] Firstly, the material was made into film samples using Cronoplast SL's Babyplast 6 / 10P micro injection molding machine for performance testing. The tensile strength and elongation at break were tested using a TSE04B universal material testing machine in accordance with the GB / 1040.3-2006 standard, and the transmittance of the sample was tested using a UV-2401PC ultraviolet spectrophotometer in accordance with the GB / T 2410-2008 standard.
[0085] According to the above test method, the samples prepared from the products of Example 1, Example 4, Example 5, Example 6, Example 7, and Comparative Examples 1 to 3 were tested, and the test results are shown in Table 2:
[0086] Table 2
[0087]
[0088]
[0089] Note: Sample thickness 0.50 mm, tensile rate 100 mm / min
[0090] From the test results shown in Table 2 above, it can be seen that the new aliphatic polycarbonate material provided by the present invention has substantially equivalent tensile strengths compared to the traditional binary polymer material CO2 / CHO (Comparative Example 1), but has higher elongation at break and significantly enhanced mechanical toughness; it has higher tensile strength than the binary polymer CO2 / ECH (Comparative Example 3), and the mechanical strength of the material is greatly improved; compared to the existing ternary polymer CO2 / CHO / PPO (Comparative Example 2), due to the effect of the polar carbon-chlorine bond, the intermolecular force is increased, thereby improving the tensile strength to a certain extent.
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A novel aliphatic polycarbonate material, characterized in that: It is polymerized by carbon dioxide, cyclohexene oxide and epoxy halogenated alkane monomers under the action of catalyst.
2. The novel aliphatic polycarbonate material according to claim 1, characterized in that: The molar ratio of the epoxy cyclohexane to the epoxy halogenated alkane monomer is 1:0.5-2.
0.
3. The novel aliphatic polycarbonate material according to claim 2, characterized in that: The epoxy haloalkane monomer is epichlorohydrin.
4. The novel aliphatic polycarbonate material according to claim 3, characterized in that: The total molar amount of cyclohexene oxide and epichlorohydrin is taken as the amount of epoxy monomer; the molar ratio of the carbon dioxide to the epoxy monomer is 0.5-1.5:
1.
5. The novel aliphatic polycarbonate material according to claim 4, characterized in that: The number average molecular weight of the material is in the range of 14,000-30,000.
6. The novel fatty carbonate material according to claim 4, characterized in that: The material has a general structure as shown in formula (V): (Ⅴ), Among them, m:n=0.5~2.0:
1.
7. The novel fatty carbonate material according to any one of claims 1 to 6, characterized in that: The catalyst is a bimetallic cobalt catalyst with a quaternary ammonium group; preferably, the catalyst has a general structure as shown in formula (VI): (Ⅵ), Wherein X is a coordinated anion group; Preferably, X is selected from 2,4-dinitrophenol oxide anion, 3,5-bis(trifluoromethyl)phenol oxide anion or trichloroacetate ion; The total molar amount of cyclohexene oxide and epichlorohydrin is taken as the amount of epoxy monomer; the molar ratio of the catalyst to the epoxy monomer is 1:2000-4000.
8. A method for preparing the novel fatty carbonate material as claimed in claim 7, characterized in that: The method comprises dissolving and mixing epoxy cyclohexane, epoxy halogenated alkane and a catalyst evenly under nitrogen protection, injecting carbon dioxide, stirring and heating, and separating and purifying after the reaction is completed to obtain the novel fatty carbonate material.
9. The method for preparing the novel fatty carbonate material according to claim 8, characterized in that: The step of charging carbon dioxide specifically includes first charging carbon dioxide to 80% of the set pressure, stirring and heating to the reaction temperature, and then charging additional carbon dioxide to 100% of the set pressure; The invention also includes timing the reaction to control the reaction conversion rate to 50%, stopping the reaction, cooling to room temperature, releasing the remaining carbon dioxide and separating and purifying the reaction product; Preferably, the separation and purification includes distilling off the unreacted alkylene oxide under reduced pressure to recover the raw materials, adding dichloromethane and 1M hydrochloric acid to the residual liquid after cooling, slowly stirring until it is evenly dissolved, adding methanol under stirring to precipitate, aging, filtering, and obtaining a pale yellow crude product, then dissolving the crude product with dichloromethane, precipitating with methanol again, repeating the process 2 to 3 times, washing, and drying, and the process is completed; Preferably, the reaction pressure is 2.0-4.0 MPa; the reaction temperature is 25-45°C; Preferably, the method further comprises first preparing the bimetallic cobalt catalyst with a quaternary ammonium group as described in claim 7.
10. Use of the novel fatty carbonate material according to any one of claims 1 to 7 in the preparation of degradable material products.
Citation Information
Patent Citations
Salen catalyst for optical polymerization reaction of racemic propylene oxide and preparation method of salen catalyst
CN102702503A
Carbon-dioxide-based polycarbonate material with optical activity as well as preparation method and application thereof
CN103524724A
Solid-phase catalyst for copolymerization of carbon dioxide / epoxy compound and preparation method of solid-phase catalyst
CN114989408A
Aliphatic polycarbonate terpolymer and preparation method thereof
CN115975166A
Zinc coordination polymer catalyst, preparation method therefor, and use thereof
WO2023217161A1
Cited By
Polycyclohexene carbonate composite material for FDM printing and preparation method thereof
CN122541977A