Composite processing aid for medical light-proof PVC (polyvinyl chloride) material and use method of composite processing aid
By using azo condensation transparent environmentally friendly organic pigments and composite calcium-zinc stabilizers and other combined additives in medical light-proof PVC materials, the problem of excessive light transmittance of light-proof PVC materials in the existing technology is solved, and a better The transparency and stability ensure the observation of liquid medicine and the quality of finished products.
Patent Information
- Application Number
- CN202411140155.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-11
AI Technical Summary
The light transmittance of existing medical light-proof PVC material processing aids is too high under light-proof conditions, resulting in the difficulty of accurately observing the liquid condition, and uneven color mixing is prone to occur during the processing, affecting the molding and use of the end product.
A medical light-proof PVC material composite processing aid composed of two azo condensation transparent and environmentally friendly organic pigments and a complex calcium and zinc stabilizer, an oxidized polyethylene homopolymer, and an acrylic processing aid is used. It is mixed in a specific ratio and mixed in the PVC Added to the material to meet the light transmittance requirements of YY 0286.3-2017.
It achieves excellent transparency and observation effects, improves the stability and plasticizing performance of PVC materials, ensures the transparency and surface quality of the product, and is suitable for the processing of medical light-proof PVC materials.
Smart Images

Figure CN118755218A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of medical devices, and in particular relates to a medical light-proof PVC material composite processing aid and a preparation method thereof. Background Art
[0002] In clinical practice, some drugs need to be infused under light-proof conditions. For example, sodium nitroprusside, nitroglycerin, and vitamin B need to use light-proof infusion sets specified in YY 0286.3-2017. The currently used medical light-proof PVC material processing aids and light-proof masterbatches have poor compatibility with the base material. The finished product is not transparent enough, and the drug solution cannot be accurately observed. During the processing, uneven color mixing is likely to occur, and the light transmittance is far beyond the standard value. Improper selection of processing aids can easily lead to poor plasticization of the base material PVC and poor fluidity, affecting the molding and use of the terminal product. Summary of the invention
[0003] In order to solve the above-mentioned problems, the present invention relates to a combination of two azo condensation transparent environmentally friendly organic pigments, a composite calcium zinc stabilizer, an oxidized polyethylene homopolymer, and an acrylic processing aid. The two azo condensation transparent environmentally friendly organic pigments are mixed in a certain proportion and added to a PVC material to make a finished product that meets the light transmittance requirements of a light-proof infusion set specified in YY 0286.3-2017.
[0004] A medical light-shielding PVC material composite processing aid comprises a light-shielding agent, a calcium-zinc heat stabilizer, a lubricant and a modifier in a weight ratio of 0.177-0.406, 1.2-1.6:0.8-1.2:2-4; specifically, the light-shielding agent is 0.177-0.406 parts by weight, the calcium-zinc heat stabilizer is 1.2-1.6 parts by weight, the lubricant is 0.8-1.2 parts by weight, and the modifier is 2-4 parts by weight.
[0005] The light-shielding agent is a mixture of 85% to 94% yellow azo condensation transparent environmentally friendly organic pigment Gumei GR yellow and 6% to 15% red azo condensation transparent environmentally friendly organic pigment Gumei 2B red. The calcium zinc heat stabilizer is a mixture of 27% to 36% by weight calcium stearate, 16% to 18% by weight zinc stearate, and 45% to 50% by weight stearyl benzoyl methane. The lubricant is an oxidized polyethylene homopolymer, and the modifier is an acrylic processing aid.
[0006] A method for using a medical light-shielding PVC material composite processing aid, the method comprising the following steps: (1) Add the light-shielding agent (such as BASF's GR Yellow and BASF's 2B Red) into the mixer according to the proportion, add the base material PVC resin powder, add the base material PVC resin powder, and observe whether the mixture is evenly mixed; (2) Add the calcium zinc heat stabilizer raw materials (calcium stearate, zinc stearate and stearyl benzoyl methane) into the mixer in proportion, mix at 900 rpm for 1 minute, and after the materials are evenly mixed, cool to room temperature, add the lubricant and modifier again, adjust the speed to 700 rpm and mix for 1 minute, and observe whether the mixture is evenly mixed without lumps; (3) The mixed materials are put into a mixer, and the PVC base material and plasticizer are added for plasticization and mixing.
[0007] A method for preparing a medical light-shielding PVC material composite processing aid, the preparation method comprising the following steps: (1) Add BASF GR Yellow and BASF 2B Red into a mixer according to the proportion, mix at 700 rpm for 2 minutes with the temperature controlled below 60°C. Observe that the mixture is evenly mixed without lumps and use as a light shielding agent for later use; (2) Add calcium stearate, zinc stearate and stearylbenzoylmethane to the mixer in proportion and mix at 900 rpm for 1 minute. After the materials are evenly mixed, cool to room temperature, add lubricant and modifier again and adjust the speed to 700 rpm and mix for 1 minute. Observe that the mixture is evenly mixed without lumps. Add light shielding agent to the mixer and mix at 600 rpm for 1 minute. (3) Observe that all the mixture is evenly mixed and becomes colorless lumps, then cool and package for later use.
[0008] The light-proof PVC material composite processing aid of the present invention not only has excellent solvent resistance, migration resistance, light fastness and heat stability, but also can maintain the brightness of monoazo pigments, and is particularly suitable for coloring plastics.
[0009] The light-shielding PVC material composite processing aid of the invention has good light-shielding effect, can effectively absorb light with a wavelength of 290-450nm, and can also have good transparency, so that the liquid level in the infusion set can be easily observed.
[0010] The light-shielding PVC material composite processing aid of the present invention can ensure that the PVC material is endowed with good stability in the later production and processing process, and the lubricant and modifier can improve the plasticizing performance of the PVC material, providing the PVC finished product with excellent transparency and surface quality in production. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is the cross section of the material ridge with the modifier added in Example 2; Figure 2 This is a cross-sectional view of the PVC material without adding a modifier in Comparative Example 1. DETAILED DESCRIPTION
[0012] The present invention will be further described below in conjunction with embodiments.
[0013] In the embodiment, the base material is selected from PVC resin powder, which is a suspension polyvinyl chloride resin with a polymerization degree of 700-2500. The plasticizer is selected from DOP or TOTM.
[0014] Example 1 Formula composition: 0.406 parts by weight of light-shielding agent, 1.2 parts by weight of composite calcium-zinc heat stabilizer, 0.8 parts by weight of lubricant, and 2 parts by weight of modifier. The light-shielding agent is a mixture of 85% to 94% by weight of BASF Gumei GR yellow and 6% to 15% by weight of BASF Gumei 2B red, the calcium-zinc heat stabilizer is a mixture of 27% to 36% by weight of calcium stearate, 16% to 18% by weight of zinc stearate, and 45% to 50% by weight of stearyl benzoyl methane; the lubricant is an oxidized polyethylene homopolymer; and the modifier is an acrylic processing aid.
[0015] Specific production steps Add BASF GR Yellow and BASF 2B Red into a mixer in proportion, add 100 parts by weight of base material PVC resin powder, mix at 700 rpm for 2 minutes, add calcium stearate, zinc stearate and stearylbenzoylmethane into the mixer in proportion, mix at 900 rpm for 1 minute, add lubricant and modifier, adjust the speed to 700 rpm and mix for 1 minute, after the above materials are mixed, they become colorless lumps, add 73 parts by weight of plasticizer DOP, after the plasticizer is fully absorbed, put the above prepared materials into a mixer, and make 0.30±0.02 thick sheets after plasticizing and mixing for standby use.
[0016] Example 2 Formula composition: 0.177 parts by weight of light-shielding agent, 1.2 parts by weight of composite calcium-zinc heat stabilizer; 1.2 parts by weight of lubricant; 4 parts by weight of modifier. The light-shielding agent is a mixture of 85% to 94% by weight of BASF Gumei GR yellow and 6% to 15% by weight of BASF Gumei 2B red, the calcium-zinc heat stabilizer is a mixture of 27% to 36% by weight of calcium stearate, 16% to 18% of zinc stearate, and 45% to 50% of stearyl benzoyl methane; the lubricant is an oxidized polyethylene homopolymer; the modifier is an acrylic processing aid.
[0017] Specific production steps Add BASF GR yellow and BASF 2B red into a mixer in proportion, add 100 parts by weight of base material PVC resin powder, mix at 700 rpm for 2 minutes, add calcium stearate, zinc stearate and stearylbenzoylmethane into the mixer in proportion, mix at 900 rpm for 1 minute, add lubricant and modifier and adjust the speed to 700 rpm and mix for 1 minute, after the above materials are mixed, they become colorless lumps, add 38 parts by weight of plasticizer DOP, and after the plasticizer is fully absorbed, put the above prepared materials into a mixer, and make 0.30±0.02 thick sheets for standby use after plasticization and mixing.
[0018] The cross-sectional view of the material ridge with the addition of the modifier in Example 2 is as follows: Figure 1 shown.
[0019] Example 3 Formula composition: 0.406 parts by weight of light-shielding color powder, 1.2 parts by weight of composite calcium-zinc heat stabilizer; 0.8 parts by weight of lubricant; 1.5 parts by weight of modifier. The light-shielding agent is a mixture of 85% to 94% by weight of BASF Gumei GR yellow and 6% to 15% by weight of BASF Gumei 2B red, the calcium-zinc heat stabilizer is a mixture of 27% to 36% by weight of calcium stearate, 16% to 18% by weight of zinc stearate, and 45% to 50% by weight of stearyl benzoyl methane; the lubricant is an oxidized polyethylene homopolymer; the modifier is an acrylic processing aid.
[0020] Specific production steps Add BASF GR yellow and BASF 2B red into a mixer in proportion, add 100 parts by weight of base material PVC resin powder, mix at 700 rpm for 2 minutes, add calcium stearate, zinc stearate and stearylbenzoylmethane into the mixer in proportion, mix at 900 rpm for 1 minute, add lubricant and modifier, adjust the speed to 700 rpm and mix for 1 minute, after the above materials are mixed, they become colorless lumps, add 79 parts by weight of plasticizer TOTM, after the plasticizer is fully absorbed, put the above prepared materials into a mixer, plasticize and mix to make 0.30±0.02 thick sheets for standby use.
[0021] Comparative Example 1 Formula composition: 0.01-0.05 parts by weight of light-shielding agent, 1 part by weight of calcium zinc heat stabilizer, and 8 parts of epoxy soybean oil. The light-shielding agent is composed of a mixture of 40%-60% by weight of iron oxide red and 20%-30% by weight of iron oxide yellow, and the calcium zinc heat stabilizer is a mixture of 27%-36% by weight of calcium ricinoleate, 16%-18% of calcium zincate, 45%-50% of zinc stearate, and 10%-15% of polyvinyl alcohol.
[0022] Specific production steps: add red iron oxide and yellow iron oxide into a mixer according to proportion, add 100 parts by weight of base material PVC resin powder, mix at 700 rpm for 2 minutes, add calcium zinc heat stabilizer into the mixer according to proportion, mix at 900 rpm for 1 minute, add epoxy soybean oil, adjust the speed to 700 rpm and mix for 1 minute, after the above materials are mixed and colorless lumps are formed, add 70 parts by weight of plasticizer DOP, after the plasticizer is fully absorbed, put the above prepared materials into a mixer, and make 0.30±0.02 thick sheets after plasticizing and mixing for stand-by use.
[0023] The cross-sectional view of the PVC material without adding modifier in Comparative Example 1 is as follows: Figure 2 shown.
[0024] Comparative Example 2 Formula composition: 0.02-0.05 parts by weight of light-shielding agent, 1.5 parts by weight of calcium zinc heat stabilizer, and 6 parts of epoxidized soybean oil. The light-shielding agent is a mixture of 15% by weight of nano zinc oxide and 85% by weight of carbon black, and the calcium zinc heat stabilizer is a mixture of 35%-40% by weight of calcium ricinoleate, 15%-20% of calcium zincate, 15%-20% of zinc stearate, and 15%-20% of polyvinyl alcohol.
[0025] Specific production steps: add nano zinc oxide and carbon black in proportion to a mixer, add 100 parts by weight of base material PVC resin powder, mix at 700 rpm for 2 minutes, add calcium zinc heat stabilizer in proportion to the mixer, mix at 900 rpm for 1 minute, add epoxy soybean oil, adjust the speed to 700 rpm and mix for 1 minute, after the above materials are mixed and colorless lumps are formed, add 80 parts by weight of plasticizer TOTM, after the plasticizer is fully absorbed, put the above prepared materials into a mixer, and make 0.30±0.02 thick sheets after plasticizing and mixing for stand-alone use.
[0026] The following implementation verification and testing of various properties were carried out using three formulation examples prepared according to the present invention and two comparative examples.
[0027] Table 1 Comparison of light-shielding properties of three embodiments It can be seen from the test results that the above test items have all reached the standards for light-proof infusion sets specified in YY 0286.3-2017, and all have a light-proof effect. However, the visible light transmittance of the comparison ratio is insufficient, which makes it impossible to effectively observe the liquid level in the device, which may easily lead to the patient not being able to replace the liquid in time after it runs out during use.
[0028] Table 2 Comparison of thermal stability of three examples It can be seen from the test results that the above test items all meet the thermal stability standards specified in GB15593-2020, but the thermal stability time of the embodiments is longer, and it is less likely to burn and discolor during product processing.
[0029] Table 3 Comparison of plasticizing properties of three embodiments As can be seen from the table above, using a torque rheometer test, after adding the patented lubricant + modifier of the present invention, the plasticizing time is significantly shortened as the amount of addition increases. from Figure 1 It can be seen that the use of the patented invention can increase the thermal stress of the material, accelerate the plasticizing ability of the material, shorten the plasticizing time, make the molding ridges smoother and eliminate bubbles in the ridges, which can significantly improve the appearance of the product.
[0030] Figure 1 and Figure 2 They are respectively the cross-sections of the material ridge (a mass of raw material squeezed out of the equipment barrel, referred to as "material ridge"). From the microscope magnified picture of the cross-section, the material with added modifier flows evenly, and the appearance of the processed product is better. The material without added modifier contains insufficient plasticized particles and bubbles, and flows unevenly, and spots and pores will appear on the appearance of the processed finished product.
[0031] The performance tests of the embodiments show that the material prepared by the composite processing aid for medical light-shielding PVC material prepared by the present invention can be processed into a light-shielding material that meets the requirements of YY0286.3-2017, replaces a single processing aid and can solve the problems of light transmittance, transparency of the terminal product and surface quality of the finished product at one time. It can be used for various medical light-shielding PVC materials.
[0032] The above descriptions are only some embodiments of the present invention and do not limit the scope of the present invention. That is, any equivalent changes or modifications made according to the contents within the scope of the present invention should be within the technical scope of the present invention.
Claims
1. A medical light-shielding PVC material composite processing aid, characterized in that: The processing aids include a light-shielding agent, a calcium-zinc heat stabilizer, a lubricant and a modifier in a weight ratio of 0.177-0.406, 1.2-1.6:0.8-1.2:2-4; The light-shielding agent is a mixture of 85-94 wt % of a yellow azo condensation type transparent environmentally friendly organic pigment and 6-15 wt % of a red azo condensation type transparent environmentally friendly organic pigment; The calcium zinc heat stabilizer is a mixture consisting of 27-36wt% calcium stearate, 16-18wt% zinc stearate, and 45-50wt% stearylbenzoylmethane.
2. The medical light-shielding PVC material composite processing aid according to claim 1, characterized in that: The lubricant is an oxidized polyethylene homopolymer; or The modifier is an acrylic processing aid.
3. The medical light-shielding PVC material composite processing aid according to claim 1, characterized in that: The yellow azo condensation type transparent environmentally friendly organic pigment is Gumei Transparent Yellow GR Yellow, and the red azo condensation type transparent environmentally friendly organic pigment is Gumei Transparent Red 2B Red.
4. The method for using a medical light-shielding PVC material composite processing aid according to any one of claims 1 to 3, characterized in that: The method of use comprises the following steps: (1) Add the light-shielding agent into the mixer according to the proportion, add the base material PVC resin powder, and observe whether the mixture is evenly mixed; (2) Add the calcium zinc heat stabilizer raw materials into the mixer in proportion. After the materials are mixed evenly, cool them to room temperature, add the lubricant and modifier again, observe whether the mixture is evenly mixed without lumps, add the plasticizer into the mixer, and wait until the plasticizer is fully absorbed; (3) The mixed materials are placed in a mixer and plasticized and mixed to obtain a medical light-proof PVC material.