Glass fiber reinforced PA66 composite material and preparation method thereof
By adding glass fiber and carbon nanotubes to PA66 composite materials and optimizing the process flow, the problem of insufficient thermal stability of PA66 composite materials in hot and humid environments has been solved, and the mechanical properties and thermal stability of the material have been significantly improved, making it suitable for many applications. application scenarios.
Patent Information
- Application Number
- CN202411055511.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing PA66 composite material has insufficient thermal stability in hot and humid environments, and the bonding strength between the glass fiber and the polyamide matrix is insufficient, which can easily lead to material breakage and performance degradation.
A method for preparing glass fiber reinforced PA66 composite materials, including a combination of PA66, styrene-butadiene transparent impact resin, glass fiber, carbon nanotubes, PA66 powder, glass fiber dispersant and compatibilizer, through drying, mixing, extrusion and Granulation process to optimize the mechanical properties and thermal stability of the material.
It improves the comprehensive performance of the material, enhances the mechanical properties and thermal stability, reduces the defects and heterogeneity of the material, improves the reliability and stability, and is suitable for applications in high load and high temperature environments.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to a glass fiber reinforced PA66 composite material and a preparation method thereof. Background Art
[0002] PA66, chemically known as poly(hexamethylene adipate), is a translucent or opaque milky white crystalline polymer with excellent mechanical properties, wear resistance, chemical resistance and processability. However, PA66 is very easy to absorb water, with a water absorption rate of about 0.25%. After absorbing water, the tensile strength and bending strength of PA66 are greatly reduced, and the performance deteriorates, which greatly limits its application. In order to expand the application of PA66, PA66 needs to be enhanced and modified. Among them, the commonly used method is glass fiber reinforcement modification. The production process uses extruder granulation. This method has the advantages of convenient processing and high production efficiency. However, after glass fiber reinforcement, there is a certain degree of floating fiber on the surface of the product, and the glass fiber on the surface of the product has poor bonding effect with thermoplastic polyurethane (TPU). Some application fields of glass fiber reinforced PA66, such as power tool housings, elevator gears, automotive parts and other fields, require TPU encapsulation bonding. In addition to requiring the glass fiber reinforced PA66 material itself to have excellent mechanical properties, thermal stability, chemical resistance and other properties, it must also have good bonding with TPU. In the prior art, when it comes to glass fiber reinforced PA66 encapsulation, a special soft alloy for nylon bonding encapsulation is usually selected for encapsulation. However, the soft alloy is often more expensive than TPU raw materials, which increases costs.
[0003] At present, the existing PA66 composite materials have insufficient thermal stability, performance degradation in hot and humid environments, and insufficient bonding strength between glass fiber and polyamide matrix. If the interface bonding is not strong, it is easy to cause material breakage and performance degradation. For this reason, a self-adhesive rubber asphalt waterproofing membrane and a production method thereof are proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a glass fiber reinforced PA66 composite material and a preparation method thereof, which solves the problems of insufficient thermal stability of the existing PA66 composite material, degradation of performance in a hot and humid environment, insufficient bonding strength between the glass fiber and the polyamide matrix, and easy breakage of the material and degradation of performance if the interface bonding is not firm, thereby meeting actual use requirements.
[0005] To achieve the above object, the present invention provides the following technical solution: a glass fiber reinforced PA66 composite material, comprising the following components in parts by weight:
[0006] 40-70 parts of PA66, 20-30 parts of butadiene-styrene transparent impact-resistant resin, 10-30 parts of glass fiber, 10-20 parts of carbon nanotubes, 8-10 parts of PA66 powder, 0.3-0.5 parts of glass fiber dispersant, 0.2-0.4 parts of compatibilizer, and 0.2-0.4 parts of lubricant.
[0007] As a preferred embodiment of the present invention, the preparation method of the glass fiber reinforced PA66 composite material comprises the following steps:
[0008] S1: PA66 and styrene-butadiene transparent impact-resistant resin are placed in a dryer for drying and mixing at a drying temperature of 80-120°C and a rotation speed of 100-300 r / min. After drying, the mixture is taken out to obtain a mixture A;
[0009] S2: The carbon nanotubes and glass fibers are placed in a dryer for drying and mixing at a drying temperature of 105-135°C and a rotation speed of 100-300 r / min. After drying, the glass fiber dispersant and compatibilizer are added to the dryer and mixed for 10-30 min after cooling to room temperature. Then, the mixture A, PA66 powder and lubricant are added and mixed for 10-20 min at a mixing temperature of 40-80°C and a rotation speed of 100-300 r / min to obtain a mixture B.
[0010] S3: Transfer the mixed material B to the extruder for extrusion at a speed of 150-300 r / min;
[0011] S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained;
[0012] S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 1 to 2 hours at a drying temperature of 80 to 125° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
[0013] As a preferred embodiment of the present invention, the melt extrusion conditions of the extruder are: zone one temperature 150-180°C, zone two temperature 180-210°C, zone three temperature 180-240°C, zone four temperature 190-240°C, zone five temperature 200-240°C, zone six temperature 200-260°C.
[0014] As a preferred embodiment of the present invention, the compatibilizer is one of modified polyamide resin, polyimide, polyether compound and polyurethane.
[0015] As a preferred embodiment of the present invention, the glass fiber adopts three specifications, and the average fiber length is 30μm-130μm, 200μm-280μm, and 320μm-450μm, and the ratio of the three specifications of glass fiber is 1:0.5-0.8:0.2.
[0016] As a preferred embodiment of the present invention, the glass fiber dispersant is one of polydimethylsiloxane and an organic dispersant containing an amide group.
[0017] As a preferred embodiment of the present invention, the lubricant is one of TAF, silicone masterbatch and polyethylene wax.
[0018] As a preferred embodiment of the present invention, the carbon nanotubes include single-walled carbon nanotubes with a diameter of 2.5 to 3 nm and a length of 8 to 20 um and multi-walled carbon nanotubes with 2 to 6 layers, an interlayer spacing of 0.43 to 0.58 nm, a diameter of 2 to 20 nm, and a length of 8 to 20 um. The ratio of the single-walled carbon nanotubes to the multi-walled carbon nanotubes is 1:0.15 to 0.3.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] Optimization of material properties: By precisely controlling the ratio of PA66, styrene-butadiene transparent impact-resistant resin, glass fiber and carbon nanotubes in the formula, the mechanical properties, heat resistance and impact resistance of the composite material can be optimized. This optimization can improve the comprehensive performance of the material and make it more suitable for various application scenarios.
[0021] Excellent dispersibility: The use of glass fiber dispersants and compatibilizers helps maintain a good dispersion state of glass fibers and carbon nanotubes. Evenly dispersed reinforcements can improve the mechanical properties of composite materials and reduce defects and heterogeneity in the material, thereby improving the reliability and stability of the material.
[0022] Improved processing performance: Adding lubricants can reduce the friction resistance of materials during extrusion, making the materials easier to process. It helps to improve production efficiency and reduce energy consumption and loss during the production process.
[0023] Enhanced mechanical properties: The introduction of reinforcing materials such as glass fiber and carbon nanotubes can significantly improve the strength and stiffness of composite materials. The materials are more suitable for applications under high loads and high stress environments, improving the reliability and service life of the materials.
[0024] Excellent thermal stability: By optimizing the melt extrusion conditions, the glass fiber reinforced PA66 composite material has excellent thermal stability. This allows the material to maintain stable performance in high temperature environments and is suitable for applications that require high temperature resistance.
[0025] Diversified applications: The use of glass fibers of different specifications and proportions, as well as different types of dispersants and lubricants, makes the composite material have more diverse performance and application potential. This diversity can meet the different requirements of different industries and application fields for material performance. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] A glass fiber reinforced PA66 composite material comprises the following components in parts by weight:
[0029] 60 parts of PA66, 20 parts of butadiene-styrene transparent impact-resistant resin, 20 parts of glass fiber, 13 parts of carbon nanotubes, 9 parts of PA66 powder, 0.4 parts of glass fiber dispersant, 0.3 parts of compatibilizer, and 0.3 parts of lubricant.
[0030] Further improved, the preparation method of the glass fiber reinforced PA66 composite material comprises the following steps:
[0031] S1: PA66 and styrene-butadiene transparent impact-resistant resin are placed in a dryer for drying and mixing at a drying temperature of 90°C and a rotation speed of 220 r / min. After drying, the mixture is taken out to obtain a mixture A;
[0032] S2: The carbon nanotubes and glass fibers were placed in a dryer for drying and mixing at a drying temperature of 115°C and a rotation speed of 240 r / min. After drying and cooling to room temperature, glass fiber dispersant and compatibilizer were added and mixed for 20 minutes. Then, mixed material A, PA66 powder and lubricant were added and mixed for 16 minutes at a mixing temperature of 60°C and a rotation speed of 240 r / min to obtain mixed material B.
[0033] S3: Transfer the mixed material B to the extruder for extrusion at a speed of 280 r / min;
[0034] S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained;
[0035] S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 1 hour at a drying temperature of 100° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
[0036] Further improved, the melt extrusion conditions of the extruder are: zone 1 temperature 160°C, zone 2 temperature 180°C, zone 3 temperature 200°C, zone 4 temperature 220°C, zone 5 temperature 220°C, zone 6 temperature 240°C.
[0037] In a further improvement, the compatibilizer is a modified polyamide resin.
[0038] As a further improvement, the glass fibers are of three specifications, and the average fiber lengths are 60 μm, 220 μm, and 350 μm, and the ratio of the three specifications of the glass fibers is 1:0.5:0.2.
[0039] In a further improvement, the glass fiber dispersant is polydimethylsiloxane.
[0040] In a further improvement, the lubricant is TAF.
[0041] In a further improvement, the carbon nanotubes include single-walled carbon nanotubes with a diameter of 2.5nm and a length of 15um and multi-walled carbon nanotubes with 4 layers, an interlayer distance of 0.48nm, a diameter of 12nm and a length of 15um. The ratio of the single-walled carbon nanotubes to the multi-walled carbon nanotubes is 1:0.18.
[0042] Example 2
[0043] A glass fiber reinforced PA66 composite material comprises the following components in parts by weight:
[0044] 40 parts of PA66, 20 parts of butadiene-styrene transparent impact-resistant resin, 10 parts of glass fiber, 10 parts of carbon nanotubes, 8 parts of PA66 powder, 0.3 parts of glass fiber dispersant, 0.2 parts of compatibilizer, and 0.2 parts of lubricant.
[0045] Further improved, the preparation method of glass fiber reinforced PA66 composite material comprises the following steps:
[0046] S1: PA66 and styrene-butadiene transparent impact-resistant resin are placed in a dryer for drying and mixing at a drying temperature of 80°C and a rotation speed of 100 r / min. After drying, the mixture is taken out to obtain a mixture A;
[0047] S2: The carbon nanotubes and glass fibers are placed in a dryer for drying and mixing at a drying temperature of 105°C and a rotation speed of 100 r / min. After drying and cooling to room temperature, glass fiber dispersant and compatibilizer are added and mixed for 10 minutes. Then, mixed material A, PA66 powder and lubricant are added and mixed for another 10 minutes at a mixing temperature of 40°C and a rotation speed of 100 r / min to obtain mixed material B.
[0048] S3: Transfer the mixed material B to the extruder for extrusion at a speed of 150 r / min;
[0049] S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained;
[0050] S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 1 hour at a drying temperature of 80° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
[0051] Further improved, the melt extrusion conditions of the extruder are: zone 1 temperature 150°C, zone 2 temperature 180°C, zone 3 temperature 180°C, zone 4 temperature 190°C, zone 5 temperature 200°C, zone 6 temperature 200°C.
[0052] In a further improvement, the compatibilizer is polyimide.
[0053] As a further improvement, the glass fibers are of three specifications, and the average fiber lengths are 30 μm, 200 μm, and 320 μm, and the ratio of the three specifications of the glass fibers is 1:0.5:0.2.
[0054] In a further improvement, the glass fiber dispersant is polydimethylsiloxane.
[0055] In a further improvement, the lubricant is TAF.
[0056] In a further improvement, the carbon nanotubes include single-walled carbon nanotubes with a diameter of 2.5nm and a length of 8um and multi-walled carbon nanotubes with 2 layers, an interlayer distance of 0.43nm, a diameter of 2nm and a length of 8um. The ratio of the single-walled carbon nanotubes to the multi-walled carbon nanotubes is 1:0.15.
[0057] Example 3
[0058] A glass fiber reinforced PA66 composite material comprises the following components in parts by weight:
[0059] 70 parts of PA66, 30 parts of butadiene-styrene transparent impact-resistant resin, 30 parts of glass fiber, 20 parts of carbon nanotubes, 10 parts of PA66 powder, 0.5 parts of glass fiber dispersant, 0.4 parts of compatibilizer, and 0.4 parts of lubricant.
[0060] Further improved, the preparation method of the glass fiber reinforced PA66 composite material comprises the following steps:
[0061] S1: PA66 and styrene-butadiene transparent impact-resistant resin are placed in a dryer for drying and mixing at a drying temperature of 120°C and a rotation speed of 300 r / min. After drying, the mixture is taken out to obtain a mixture A;
[0062] S2: The carbon nanotubes and glass fibers were placed in a dryer for drying and mixing at a drying temperature of 135°C and a rotation speed of 300 r / min. After drying and cooling to room temperature, glass fiber dispersant and compatibilizer were added and mixed for 30 minutes. Then, mixed material A, PA66 powder and lubricant were added and mixed for 20 minutes at a mixing temperature of 80°C and a rotation speed of 300 r / min to obtain mixed material B.
[0063] S3: Transfer the mixed material B to the extruder for extrusion at a speed of 300 r / min;
[0064] S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained;
[0065] S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 2 hours at a drying temperature of 125° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
[0066] Further improved, the melt extrusion conditions of the extruder are: zone one temperature 180°C, zone two temperature 210°C, zone three temperature 240°C, zone four temperature 240°C, zone five temperature 240°C, zone six temperature 260°C.
[0067] In a further improvement, the compatibilizer is a modified polyamide resin.
[0068] As a further improvement, the glass fibers are of three specifications, and the average fiber lengths are 130 μm, 280 μm, and 450 μm, and the ratio of the three specifications of the glass fibers is 0.8:0.2.
[0069] In a further improvement, the glass fiber dispersant is one of polydimethylsiloxane and an organic dispersant containing an amide group.
[0070] In a further improvement, the lubricant is polyethylene wax.
[0071] In a further improvement, the carbon nanotubes include single-walled carbon nanotubes with a diameter of 3nm and a length of 20um and multi-walled carbon nanotubes with 6 layers, an interlayer distance of 0.58nm, a diameter of 20nm and a length of 20um. The ratio of single-walled carbon nanotubes to multi-walled carbon nanotubes is 1:0.3.
[0072] Example 4
[0073] A glass fiber reinforced PA66 composite material comprises the following components in parts by weight:
[0074] 60 parts of PA66, 20 parts of glass fiber, 9 parts of PA66 powder, 0.4 parts of glass fiber dispersant, 0.3 parts of compatibilizer, and 0.3 parts of lubricant.
[0075] Further improved, the preparation method of glass fiber reinforced PA66 composite material comprises the following steps:
[0076] S1: PA66 is placed in a dryer for drying and mixing at a drying temperature of 90°C and a rotation speed of 220 r / min. After drying, the mixture is taken out to obtain a mixture A;
[0077] S2: The carbon nanotubes and glass fibers were placed in a dryer for drying and mixing at a drying temperature of 115°C and a rotation speed of 240 r / min. After drying and cooling to room temperature, glass fiber dispersant and compatibilizer were added and mixed for 20 minutes. Then, mixed material A, PA66 powder and lubricant were added and mixed for 16 minutes at a mixing temperature of 60°C and a rotation speed of 240 r / min to obtain mixed material B.
[0078] S3: Transfer the mixed material B to the extruder for extrusion at a speed of 280 r / min;
[0079] S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained;
[0080] S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 1 hour at a drying temperature of 100° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
[0081] Further improved, the melt extrusion conditions of the extruder are: zone 1 temperature 160°C, zone 2 temperature 180°C, zone 3 temperature 200°C, zone 4 temperature 220°C, zone 5 temperature 220°C, zone 6 temperature 240°C.
[0082] In a further improvement, the compatibilizer is a modified polyamide resin.
[0083] In a further improvement, the glass fiber dispersant is polydimethylsiloxane.
[0084] In a further improvement, the lubricant is TAF.
[0085] According to the above process steps, glass fiber reinforced PA66 composite splines were prepared and vertical combustion performance tests, limiting oxygen index tests and mechanical performance tests were carried out. The vertical combustion performance test is specifically as follows: CZF-3 horizontal vertical combustion tester is used to test according to GB / T2408-2008 standard, and the spline size is 13mmX80mmX3.2mm. The mechanical performance test is specifically as follows: the tensile performance is tested according to GB / T1040.2-2006, the spline size is 150mmX20mmX4mm, and the running speed is 50mm / min; the bending performance is tested in accordance with GB / T9341-2008, the spline size is 80mmX10mmX4mm, and the running speed is 3mm / min; the impact performance is tested in accordance with GB / T1843-2008, and the spline size is 80mmX10mmX4mm. See the table below for detailed results:
[0086] Sample No. Is there any dripping Tensile strength / MPa Bending strength / MPa <![CDATA[Impact strength / (KJ / m 2 )]]> Example 1 none 129.29 177.72 8.50 Example 2 none 127.16 177.15 8.22 Example 3 none 106.64 158.25 7.23 Example 4 (Comparative) have 90.37 120.22 6.69
[0087] In Examples 1-3, transparent styrene-butadiene impact-resistant resin, three glass fibers with different fiber lengths, and carbon nanotubes were added, so that the flame retardancy, tensile strength, flexural strength, and impact strength of the composite materials prepared therefrom were significantly improved.
[0088] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A glass fiber reinforced PA66 composite material, characterized in that: The invention comprises the following components in parts by weight: 40-70 parts of PA66, 20-30 parts of butadiene-styrene transparent impact-resistant resin, 10-30 parts of glass fiber, 10-20 parts of carbon nanotubes, 8-10 parts of PA66 powder, 0.3-0.5 parts of glass fiber dispersant, 0.2-0.4 parts of compatibilizer, and 0.2-0.4 parts of lubricant.
2. The method for preparing a glass fiber reinforced PA66 composite material according to claim 1, characterized in that: The preparation method of the glass fiber reinforced PA66 composite material comprises the following steps: S1: PA66 and styrene-butadiene transparent impact-resistant resin are placed in a dryer for drying and mixing at a drying temperature of 80 to 120°C and a rotation speed of 100 to 300 r / min. After drying, the mixture is taken out to obtain a mixture A; S2: The carbon nanotubes and glass fibers are placed in a dryer for drying and mixing at a drying temperature of 105-135°C and a rotation speed of 100-300 r / min. After drying, the glass fiber dispersant and compatibilizer are added to the dryer and mixed for 10-30 min after cooling to room temperature. Then, the mixture A, PA66 powder and lubricant are added and mixed for 10-20 min at a mixing temperature of 40-80°C and a rotation speed of 100-300 r / min to obtain a mixture B. S3: Transfer the mixed material B to the extruder for extrusion at a speed of 150-300 r / min; S4: cooling the extruded melt through a continuous cold water tank, wherein the first half of the continuous cold water tank is a circulating water tank and the second half is a static cold water tank, and after cooling, a glass fiber reinforced PA66 composite is obtained; S5: The glass fiber reinforced PA66 composite material obtained after cooling is granulated by using a pelletizer, and the granulated material is placed in a dryer for drying for 1 to 2 hours at a drying temperature of 80 to 125° C. After drying, the glass fiber reinforced PA66 composite particles are obtained.
3. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The melt extrusion conditions of the extruder are: zone 1 temperature 150-180°C, zone 2 temperature 180-210°C, zone 3 temperature 180-240°C, zone 4 temperature 190-240°C, zone 5 temperature 200-240°C, zone 6 temperature 200-260°C.
4. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The compatibilizer is one of modified polyamide resin, polyimide, polyether compound and polyurethane.
5. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The glass fibers are of three specifications, and the average fiber lengths are 30 μm to 130 μm, 200 μm to 280 μm, and 320 μm to 450 μm. The ratio of the three specifications of the glass fibers is 1:0.5 to 0.8:0.
2.
6. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The glass fiber dispersant is one of polydimethylsiloxane and an organic dispersant containing an amide group.
7. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The lubricant is one of TAF, silicone masterbatch and polyethylene wax.
8. The method for preparing a glass fiber reinforced PA66 composite material according to claim 2, characterized in that: The carbon nanotubes include single-walled carbon nanotubes with a diameter of 2.5-3nm and a length of 8-20um and multi-walled carbon nanotubes with 2-6 layers, an interlayer distance of 0.43-0.58nm, a diameter of 2-20nm and a length of 8-20um. The ratio of single-walled carbon nanotubes to multi-walled carbon nanotubes is 1:0.15-0.3.
Citation Information
Patent Citations
Carbon nano tube reinforced nylon-based composite material and preparation method therefor
CN104974508A
Heat conductive plastic and preparation method thereof
CN108342073A
Carbon nanotube reinforced and modified nylon material and preparation method thereof
CN113337108A
Modified PA66 material as well as preparation method and application thereof
CN115216144A