Super-infiltration CuS-coated SiO2 photo-thermal composite material as well as preparation method and application thereof
By coating the surface of CuS nanoparticles with SiO2 and introducing low surface energy substances, a super-wetting CuS@SiO2 photothermal composite material is formed, which solves the problem of retention and durability of CuS in the field of photothermal conversion and achieves efficient seawater desalination and prevention. Ice effect and reduced costs.
Patent Information
- Application Number
- CN202411008693.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-26
AI Technical Summary
In the existing technology, CuS as a photothermal conversion material in the fields of seawater desalination and anti-icing has problems such as difficulty in effectively staying at the air-seawater interface for gas-liquid conversion, environmental pollution, and poor wear and weather resistance, and the cost is high.
By preparing CuS nanoparticles with good localized surface plasmon resonance performance, coating the surface with SiO2, and introducing silane low surface energy substances for modification, a super-wetting CuS@SiO2 photothermal composite material is formed, which can be used for photothermal anti-icing. De-icing areas and desalination.
It realizes the efficient application of CuS in the field of photothermal conversion, improves the durability and cost-effectiveness of the material, and shows excellent wear resistance, weather resistance and self-cleaning performance in the anti-icing field.
Smart Images

Figure HDA0004963682750000011 
Figure HDA0004963682750000012 
Figure HDA0004963682750000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional materials, and in particular relates to a super-wettable CuS@SiO2 photothermal composite material and a preparation method and application thereof. Background Art
[0002] Traditional desalination technologies, such as reverse osmosis, multi-stage flash evaporation, multi-effect distillation, and electrodialysis, consume a large amount of fossil energy, increase operating costs, and cause environmental pollution. As a new desalination process, solar-driven interfacial photothermal evaporation (SDIE) converts solar energy into thermal energy through photothermal conversion materials, achieves rapid local heat positioning at the air-water interface, and can significantly improve the energy utilization efficiency in the gas-liquid conversion process; it has good application prospects in the field of solar-driven water treatment.
[0003] On the other hand, as an inevitable natural phenomenon, the hazards of ice accumulation have widely affected agriculture, animal husbandry, aviation, electrified railway systems and other fields. Traditional deicing technologies include thermal deicing, mechanical deicing, liquid deicing and other methods, which have the disadvantages of high power consumption, low deicing efficiency, low safety, and environmental pollution. The construction of superhydrophobic surfaces can overcome the shortcomings of the above traditional methods and is considered to be one of the most promising anti-icing technologies. In recent years, the combination of photothermal materials and superhydrophobic materials to manufacture photothermal superhydrophobic surfaces for application in the field of anti-icing has received widespread attention; however, most of the existing methods have the disadvantages of expensive raw materials, complex equipment, and weak wear resistance, weather resistance and aging resistance of the products. Therefore, the further development of superhydrophobic photothermal composite anti-icing materials with simple preparation process, low cost and excellent comprehensive performance is a hot topic of current research.
[0004] As a new type of plasma resonance nanomaterial, CuS has a strong near-infrared plasma resonance effect and a wide absorption band. It can provide high photothermal conversion efficiency and long-term durability, and has the advantages of low cost, low toxicity, high purity, good biocompatibility, and excellent photostability. It is a promising photothermal conversion material. However, CuS is difficult to dissolve in most solvents. In the field of photothermal water evaporation, if CuS particles are directly used for seawater desalination or wastewater treatment, they cannot effectively stay at the air-seawater interface for normal gas-liquid conversion process, and it is difficult to achieve efficient photothermal conversion efficiency. The material cannot be recycled during or after use, causing environmental pollution. In addition, in the field of photothermal anti-icing, CuS particles, as metal sulfides, are difficult to directly modify with low surface energy materials to achieve superhydrophobic properties. Summary of the invention
[0005] The main purpose of the present invention is to provide a simple, easy and scalable super-wettable CuS@SiO2 photothermal composite material in view of the shortcomings of the prior art. First, CuS nanoparticles with good local surface plasma resonance performance are prepared, and then SiO2 is coated on the surface of the CuS nanoparticles, and silane low surface energy substances are further introduced to modify the surface. The obtained CuS@SiO2 photothermal composite material has good super-wettability, near-infrared plasma resonance performance and photothermal conversion effect. The prepared super-hydrophobic CuS@SiO2 photothermal coating can be applied to the field of photothermal anti-icing and de-icing. The prepared super-wettable Janus structure water evaporator has good solar-driven synchronous photocatalytic purification and photothermal water evaporation performance, and has great potential application value in the fields of sewage treatment and seawater desalination.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a super-wettable CuS@SiO2 photothermal composite material comprises the following steps:
[0008] (1) sulfur powder, octadecene (ODE), and oleylamine (OM) are sequentially added to a reaction vessel, and a first heating reaction is performed under vacuum conditions to obtain an orange-red transparent S precursor solution;
[0009] (2) Cool the S precursor solution to room temperature by introducing a protective atmosphere (such as Ar gas), then add copper salt, conduct a second heating reaction under vacuum conditions, and then cool to room temperature by introducing a protective atmosphere (such as Ar gas) to obtain a black-green CuS dispersion.
[0010] (3) The CuS dispersion obtained in step (2) is subjected to centrifugal separation using alcohol solvent I as a detergent to obtain a CuS nanocrystal precipitate; then toluene is added to uniformly disperse the precipitate to obtain a CuS-toluene dispersion;
[0011] (4) adding the CuS-toluene dispersion obtained in step (3) to the alcohol solvent II under magnetic stirring conditions, stirring the dispersion to uniformly disperse the CuS and volatilize the toluene;
[0012] (5) adding an alkali solution and a hydrolyzable silicon source to the dispersion obtained in step (4) in sequence, and continuing to react by stirring to obtain a super-hydrophilic CuS@SiO2 photothermal composite material;
[0013] (6) Adding a silane-based low surface energy material to the reaction system obtained in step (5), continuing the stirring reaction, and obtaining a super-hydrophobic CuS@SiO2 photothermal composite material.
[0014] In the above scheme, the super wettability is super hydrophilicity and / or super hydrophobicity. The super hydrophilic CuS@SiO2 photothermal composite material and the super hydrophobic CuS@SiO2 photothermal composite material obtained in steps (5) and (6) respectively are both super wettability CuS@SiO2 photothermal composite materials, which are mainly composed of nano CuS@SiO2 particles and nano SiO2 particles.
[0015] In the above scheme, the copper salt can be selected from one or more of copper acetate monohydrate, copper nitrate dihydrate and the like.
[0016] In the above scheme, the CuS nanocrystal precipitate has a nanosheet structure, and the sheet diameter is 10 to 30 nm.
[0017] In the above scheme, the hydrolyzable silicon source can be selected from one or more of tetraethyl orthosilicate, tetrabutyl orthosilicate, etc.
[0018] In the above scheme, the silane-based low surface energy material can be selected from one or more of hexamethyldisilazane (HMDS), methyltriethoxysilane (MTES), hexadecyltrimethoxysilane (HDTMS) and the like.
[0019] In the above scheme, the solution system obtained in step (5) is directly sprayed on the surface of the substrate and dried to obtain a super-hydrophilic CuS@SiO2 composite coating.
[0020] In the above scheme, the solution system obtained in step (6) is directly sprayed on the surface of the substrate and dried to obtain a super-hydrophobic CuS@SiO2 composite coating.
[0021] In the above scheme, the heating rates of steps (1) to (2) are both 8 to 10°C / min.
[0022] In the above scheme, the temperature of the first heating reaction in step (1) is 90-100° C. and the time is 20-40 min.
[0023] In the above scheme, the temperature used for the second heating reaction in step (2) is 150-220° C. and the time is 20-40 min.
[0024] In the above scheme, the temperature used in steps (3) to (6) is room temperature.
[0025] In the above scheme, in step (3), the rotation speed used for centrifugal separation is 3500-4500 rpm and the centrifugal time is 4-6 min.
[0026] In the above scheme, the alcohol solvent I in step (3) is one of methanol, ethanol, and ethanol / acetone mixed solvent.
[0027] In the above scheme, the alcohol solvent II in step (4) is one of methanol, ethanol, isopropanol, etc.
[0028] In the above scheme, the alkali solution in step (5) is a NaOH aqueous solution or ammonia water, wherein the NaOH concentration is 1-1.8 mol / L, and the ammonia concentration is 25-29 wt%.
[0029] In the above scheme, the molar ratio of sulfur powder and copper salt in steps (1) to (2) is 2:1.
[0030] In the above scheme, the volume ratio of octadecene to oleylamine in steps (1) to (2) is 4:(1 to 4).
[0031] In the above scheme, the concentration of CuS in the CuS-toluene dispersion is (0.10-0.15) g / mL.
[0032] In the above scheme, the volume ratio of the CuS-toluene dispersion, alcohol solvent II, alkali solution, hydrolyzable silicon source, and silane-based low surface energy substance in steps (4) to (6) is (1-5):(5-7):(0.2-0.4):(1-1.4):(0.6-1).
[0033] In the above scheme, the stirring treatment time of step (4) is 0.5 to 1 h.
[0034] In the above scheme, the stirring reaction time of step (5) is 20 to 24 hours.
[0035] In the above scheme, the stirring reaction time of step (6) is 6 to 12 hours.
[0036] The present invention also provides a CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure prepared by using the above-mentioned super-wet CuS@SiO2 photothermal composite material, and the specific preparation steps include:
[0037] The super-hydrophobic aqueous solution system obtained in step (5) is sprayed on the upper surface of the foam substrate, and the super-hydrophilic aqueous solution system obtained in step (6) is immersed in the lower surface of the foam substrate. After drying, a CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure is obtained.
[0038] The present invention also provides a photothermal composite anti-icing coating prepared by using the above-mentioned super-wettable CuS@SiO2 photothermal composite material, and the specific preparation steps include:
[0039] 1) Under stirring conditions, hydroxy acrylic resin, fluorocarbon resin, alkyd resin, polypropylene resin, silane coupling agent, and filler are added to an organic solvent (butyl acetate, etc.) in sequence, and stirred (12 to 24 hours) to obtain a resin primer;
[0040] 2) On the surface of the glass substrate, first spray the resin primer obtained in step 1) as a binder to improve the wear resistance and weather resistance of the coating, and then spray the super-hydrophobic CuS@SiO2 photothermal composite coating when the primer reaches surface dryness, and dry to obtain the super-hydrophobic CuS@SiO2 photothermal anti-icing coating.
[0041] In the above scheme, the mass ratio of the hydroxy acrylic resin, fluorocarbon resin, alkyd resin and polypropylene resin is (80-90):(15-20):(40-45):(10-15).
[0042] In the above scheme, the mass ratio of the hydroxy acrylic resin to the organic solvent is 90:(250-300).
[0043] In the above scheme, the volume ratio of the silane coupling agent to the organic solvent is (0.5-2):100.
[0044] In the above scheme, the mass ratio of the filler to the resin introduced into the resin primer (the sum of acrylic resin, fluorocarbon resin, alkyd resin and polypropylene resin) is (10-15): (155-170).
[0045] The super-wetting CuS@SiO2 photothermal composite material prepared according to the above scheme has excellent super-wetting performance, near-infrared plasma resonance performance, high photothermal conversion efficiency and long-term durability. The super-hydrophobic CuS@SiO2 photothermal composite coating is used in combination with a resin primer to construct a photothermal composite anti-icing coating on a substrate. This anti-icing coating has wear resistance, weather resistance, long-term stable photothermal performance, and certain anti-fouling, self-cleaning, anti-corrosion and other functions; it is suitable for the field of photothermal anti-icing.
[0046] On the other hand, since the super-wettable CuS@SiO2 photothermal composite coating (super-hydrophobic and super-hydrophilic coatings) has excellent super-wetting properties, high photothermal conversion efficiency and photocatalytic degradation performance, it can be combined with a porous substrate to prepare a CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure, which has excellent simultaneous photocatalytic purification and photothermal water evaporation performance, and has outstanding self-floating, self-cleaning and vapor diffusion functions, and is suitable for seawater desalination and treatment of dye wastewater.
[0047] The principle of the present invention is:
[0048] First, CuS nanoparticles with good localized surface plasmon resonance performance are prepared. Then, they are added into an alkaline solution of a hydrolyzable silicon source and stirred to react. SiO2 is coated on the surface of the CuS nanoparticles. The resulting composite material is further surface modified with a silane-based low surface energy substance to regulate its wetting properties, thereby obtaining superhydrophilic and superhydrophobic CuS@SiO2 photothermal composite materials, respectively.
[0049] The present invention uses a super-hydrophobic CuS@SiO2 photothermal composite coating and a resin primer to construct a photothermal composite anti-icing coating on a substrate, which has a micro-nano hierarchical structure: the super-hydrophobic CuS@SiO2 coating is deposited on the surface of the resin primer of the present invention, so that the surface of the obtained anti-icing coating further grows a micron-sized papillary composite sediment, and the particle size of the micron-sized papillary composite sediment is concentrated between 70 and 100 μm, mainly composed of nano-sized CuS@SiO2 composite nanoparticles and SiO2 nanoparticles. The present invention combines the surface modification of low-surface energy materials with the construction method of micro-nano structures. The constructed low-surface energy micro-nano rough structure enables the CuS@SiO2 anti-icing coating to have excellent super-hydrophobicity and wear resistance and weather resistance, and can also promote the copper sulfide photothermal nanoparticles to be stably embedded in the substrate, further ensuring the long-term stability of the photothermal performance of the obtained composite coating. In addition, the excellent super-hydrophobic performance makes the anti-icing coating also have certain anti-fouling, self-cleaning, anti-corrosion and other functions.
[0050] The present invention combines the obtained super-hydrophilic and super-hydrophobic CuS@SiO2 photothermal composite material with a porous substrate to prepare a CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure. On the one hand, the excellent super-hydrophobicity of the upper layer of the evaporator makes the evaporator have excellent self-floating properties, avoiding the problems that the hydrophobic agent easily falls off or oxidatively decomposes under strong light and loses floatability caused by the introduction of hydrophobic agents and external supports to make the evaporator floatable, and the addition of supporting substrates is not conducive to the conduction of salt and the transportation of water. On the other hand, the lower layer of the evaporator has excellent super-hydrophilicity to ensure sufficient water supply, and seawater can be continuously sucked from the lower layer to the liquid surface for vapor-liquid exchange process. In addition, the evaporator of the present invention has self-cleaning performance, which can use non-irradiation time to eliminate crystallized salts on the surface and inside of the evaporator without affecting the normal use during irradiation, greatly improving the energy utilization efficiency of the evaporator for solar energy.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1) In view of the limitations of CuS in the application of photocatalysis, photothermal deicing and other fields, the present invention proposes for the first time to first coat SiO2 on its surface, and then use a low surface energy material to modify its surface to finally obtain super-hydrophilic and super-hydrophobic CuS@SiO2 photothermal composite materials, which can effectively improve the application limitations of CuS in various fields such as photocatalysis and photothermal deicing;
[0053] 2) The CuS@SiO2 photothermal composite material of the present invention has high near-infrared photothermal conversion efficiency, high chemical stability, low cost, simple preparation method, and can be prepared in large quantities, and has great application prospects;
[0054] 3) The super-hydrophobic CuS@SiO2 photothermal composite coating prepared by the present invention can achieve the synergistic effect of active deicing and passive anti-icing in the field of photothermal anti-icing / deicing, and has good wear resistance and weather resistance; the prepared super-hydrophobic / super-hydrophilic Janus structure CuS@SiO2 photothermal water evaporator has low cost, can simultaneously and efficiently realize the two functions of photothermal evaporation of water and photocatalytic degradation of dye solution, and can be applied to fields such as seawater desalination and wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a morphology photograph of the super-hydrophobic CuS@SiO2 photothermal composite coating obtained in Example 1.
[0056] Figure 2 This is a contact angle photograph of the super-hydrophobic CuS@SiO2 photothermal composite coating obtained in Example 1.
[0057] Figure 3 This is the TEM characterization image of the super-hydrophobic CuS@SiO2 photothermal composite material obtained in Example 1.
[0058] Figure 4 This is the absorption curve of the super-hydrophobic CuS@SiO2 photothermal composite material obtained in Example 1.
[0059] Figure 5 This is the XRD curve diagram of the super-hydrophobic CuS@SiO2 photothermal composite material obtained in Example 1.
[0060] Figure 6 This is the FTIR curve of the super-wettable CuS@SiO2 photothermal composite material obtained in Example 1.
[0061] Figure 7 The super-hydrophobic CuS@SiO2 photothermal composite coating obtained in Example 1 was 2 Below is a graph showing the surface temperature changing with time.
[0062] Figure 8 This is a morphology photograph of the Janus-structured CuS@SiO2 photothermal water evaporator prepared in Example 3.
[0063] Fig. 9 This is a contact angle photograph of the Janus-structured CuS@SiO2 photothermal water evaporator prepared in Example 3.
[0064] Fig.10 This is the morphology of the CuS@SiO2 photothermal composite anti-icing coating sample and the super-hydrophobic SiO2 coating sample described in Application Example 1.
[0065] Fig.11 This is the SEM photo of the CuS@SiO2 photothermal composite anti-icing coating sample described in Application Example 1.
[0066] Fig.12 The CuS@SiO2 photothermal composite anti-icing coating sample and the ordinary super-hydrophobic SiO2 coating sample described in Application Example 1 were tested under a light intensity of 0.5 kW / m 2 , comparison chart of delayed freezing time at different temperatures.
[0067] Fig.13 This is a comparison chart of the delayed freezing time of the CuS@SiO2 photothermal composite anti-icing coating sample described in Application Example 1 and the ordinary superhydrophobic SiO2 coating sample at -20°C and different light intensities.
[0068] Fig.14 The CuS@SiO2 photothermal composite anti-icing coating sample described in Application Example 1 and the ordinary super-hydrophobic SiO2 coating sample were subjected to -15℃ and 1kW / m 2 Comparison of morphologies of ice melting process under different light intensities.
[0069] Fig.15 This is the surface morphology and contact angle comparison diagram of the CuS@SiO2 photothermal composite anti-icing coating sample before and after the wear resistance experiment described in Application Example 1.
[0070] Fig.16 This is a before and after comparison of the Janus structure CuS@SiO2 water evaporator described in Application Example 2 degrading sodium chloride-methylene blue dye solution.
[0071] Fig.17 This is a comparison chart of the mass loss of seawater simulated by the Janus structure CuS@SiO2 water evaporator described in Application Example 2 and melamine foam (MF).
[0072] Fig.18 This is a comparison chart of the absorbance changes of the dye solution caused by the Janus structure CuS@SiO2 water evaporator and MF described in Application Example 2 within two hours. DETAILED DESCRIPTION
[0073] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples. These descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.
[0074] Example 1
[0075] A super-hydrophobic CuS@SiO2 photothermal composite material and coating, wherein the preparation method thereof comprises the following steps:
[0076] 1) Weigh 0.256 g sulfur powder (8 mmol) into a 50 mL three-necked flask, add 40 mL octadecene (ODE) and 10 mL oleylamine (OM) in sequence, and heat to 90 °C at a rate of 10 °C / min under vacuum conditions, and keep at this temperature for 30 min to obtain an orange-red transparent S precursor solution;
[0077] 2) Ar gas was introduced and the obtained S precursor solution was cooled to room temperature, and then 0.799 g of copper acetate monohydrate Cu(Ac)2·H2O (4 mmol) was added, and vacuum was applied at room temperature for 30 min, and then the temperature was raised to 200°C at a rate of 10°C / min, and kept at this temperature for 30 min to obtain a black-green dispersion; the mixture was further cooled to room temperature under Ar atmosphere to obtain a CuS black-green dispersion (concentration of 0.008 M);
[0078] 3) washing the CuS dispersion obtained in step 2) twice with methanol as a detergent by centrifuging (4000 rpm, 5 min) to separate the nanocrystal precipitate, and then adding toluene to evenly disperse the precipitate to obtain a CuS-toluene dispersion, wherein the solid-liquid ratio of the CuS nanocrystal precipitate to toluene is 0.13 g / mL;
[0079] 4) Under magnetic stirring, take 6 mL of the CuS-toluene dispersion obtained in step 3), slowly pour it into 25 mL of ethanol and stir for 30 min to make it evenly dispersed and evaporate the toluene;
[0080] 5) Add 1.5 mL of NaOH solution (1.8 mol / L) and 5 mL of ethyl orthosilicate to the mixed solution obtained in step 4) in sequence, and stir for 24 h;
[0081] 6) Add 5.0 mL of hexamethyldisilazane (HMDS) to the solution system in step 5) and continue stirring for 12 h to obtain a super-hydrophobic CuS@SiO2 photothermal composite coating;
[0082] 7) Spray the coating obtained in step 6) on the surface of the substrate and dry it to obtain a super-hydrophobic CuS@SiO2 photothermal composite coating.
[0083] Figure 1 , 2The morphology photos and contact angle photos of the coating sample obtained in this embodiment are respectively, and the results show that the methyl blue droplet can "stand" well on the coating surface, and the measured water contact angle is 156°. The obtained coating sample exhibits good superhydrophobic performance.
[0084] Figure 3 The transmission electron microscope (TEM) image of the coating solution (step 6) obtained in this embodiment) shows that the hydrolyzable silicon source is in situ hydrolyzed in the presence of flaky CuS nanocrystals and alkaline solution, and then modified with a low surface energy substance to obtain a super-hydrophobic CuS@SiO2 nanocomposite material (as shown in Figures a and b). The prepared CuS@SiO2 nanocomposite material is composed of amorphous SiO2 and CuS phases, including CuS@SiO2 nanoparticles and SiO2 nanoparticles, wherein the typical microscopic morphology of the CuS@SiO2 nanoparticles is that the amorphous low surface energy SiO2 in situ covers the flaky CuS phase to obtain a core-shell structure (as shown in Figures c and d).
[0085] Figure 4 This is the UV-visible absorption spectrum of the coating solution obtained in this example. The sample has a strong absorption peak in the near-infrared (its peak is at 1200-1400nm), which indicates that the synthesized photothermal composite coating has a strong near-infrared localized surface plasmon resonance performance.
[0086] Figure 5 The XRD diagram of the coating obtained in this example shows that the diffraction peak of CuS contained in the coating is consistent with the result of the copper blue (CuS) spectrum (JCPDS 00-06-0464). Therefore, it can be known that in the composite coating prepared by the present invention, the nanocrystalline component coated by SiO2 is CuS.
[0087] Figure 6 The FTIR spectrum of the super hydrophobic CuS@SiO2 coating is at 845, 1254, 2852 and 2961 cm -1 Absorption peaks appeared at 845 and 1254 cm -1 The absorption bands at 2961cm -1 Corresponding to the stretching vibration of -CH3 group, located at 2852cm -1 The peak of 960cm is the symmetric stretching vibration of CH chain, indicating that the hydrophilic group Si-OH on the surface of SiO2 in the coating obtained in this example is replaced by the hydrophobic group Si-CH3. -1 The peak at belongs to the bending vibration peak of Si-OH bond. The Si-OH peak indicates that the super-hydrophilic CuS@SiO2 sample has a terminal hydroxyl surface and good super-hydrophilicity.
[0088] Figure 7 The model is CEL-S500-T5, and the light intensity is 1kW / m 2 A xenon lamp (1 sun) was used to irradiate the composite coating prepared in this example and the glass substrate without coating at the same time, and a thermocouple was used to record the temperature change in real time to test its light-to-heat conversion performance. Figure 6 It can be seen that under the illumination of 1 sun, the temperature of the CuS@SiO2 composite coating increased from 21°C to 75°C within 250 seconds, an increase of 54°C; while the temperature of the glass substrate only increased to 36°C, an increase of only 15°C. It can be seen that the CuS@SiO2 coating prepared by the present invention has a good light-to-heat conversion effect.
[0089] Example 2
[0090] A super-hydrophobic CuS@SiO2 photothermal composite material and coating, wherein the preparation method thereof comprises the following steps:
[0091] 1) Weigh 0.256 g sulfur powder (8 mmol) into a 50 mL three-necked flask, add 40 mL octadecene (ODE) and 10 mL oleylamine (OM) in sequence, and heat to 90 °C at a rate of 10 °C / min under vacuum conditions, and keep at this temperature for 30 min to obtain an orange-red transparent S precursor solution;
[0092] 2) Ar gas was introduced and the obtained S precursor solution was cooled to room temperature, and then 0.799 g of copper acetate monohydrate Cu(Ac)2·H2O (4 mmol) was added, and vacuum was applied at room temperature for 30 min, and then the temperature was raised to 200°C at a rate of 10°C / min, and kept at this temperature for 30 min to obtain a black-green dispersion; the mixture was further cooled to room temperature under Ar atmosphere to obtain a CuS black-green dispersion (concentration of 0.008 M);
[0093] 3) washing the CuS dispersion obtained in step 2) twice with methanol as a detergent by centrifuging (4000 rpm, 5 min) to separate the nanocrystal precipitate, and then adding toluene to evenly disperse the precipitate to obtain a CuS-toluene dispersion, wherein the solid-liquid ratio of the CuS nanocrystal precipitate to toluene is 0.13 g / mL;
[0094] 4) Under magnetic stirring, take 6 mL of the CuS-toluene dispersion obtained in step 3), slowly pour it into 25 mL of ethanol and stir for 30 min to make it evenly dispersed and evaporate the toluene;
[0095] 5) Add 2 mL of aqueous ammonia solution (26 wt%) and 4 mL of butyl orthosilicate to the mixed solution obtained in step 4) in sequence, and stir for 24 h;
[0096] 6) Add 1 mL of hexadecyltrimethoxysilane (HDTMS) to the solution system in step 5) and continue stirring for 12 h to obtain a super-hydrophobic CuS@SiO2 photothermal composite coating;
[0097] 7) Spray the coating obtained in step 6) on the surface of the substrate and dry it to obtain a super-hydrophobic CuS@SiO2 photothermal composite coating.
[0098] Example 3
[0099] A CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure, and a preparation method thereof comprises:
[0100] 1) Prepare a super-hydrophobic CuS@SiO2 photothermal composite material by referring to steps 1) to 6) of Example 1;
[0101] 2) Prepare a super-hydrophilic CuS@SiO2 photothermal composite material by referring to steps 1) to 5) of Example 1;
[0102] 3) Prepare melamine foam (hereinafter referred to as MF) and cut it into square pieces (area 2.5×2.5cm 2 , thickness is 0.5 cm), and 1 mL of superhydrophobic CuS@SiO2 photothermal composite material is sprayed on the upper surface of MF, and 2.5 mL of superhydrophilic CuS@SiO2 material is taken and the lower surface of MF is immersed therein to make it fully absorbed, and then dried to obtain the superhydrophobic / superhydrophilic Janus structure CuS@SiO2 photothermal water evaporator.
[0103] The morphology photos and upper surface contact angle photos of the obtained CuS@SiO2 photothermal water evaporator are shown in the figure. Figure 8 , 9 As shown in the figure, the methylene blue droplets can "stand" well on the upper surface of the water evaporator, and the water contact angle of the upper surface is measured to be 155°. The obtained coating sample shows good superhydrophobic properties.
[0104] Application Example 1
[0105] According to the preparation method described in Example 1, a super-hydrophobic CuS@SiO2 composite photothermal coating is prepared and applied to the anti-icing field. The solution system obtained in step 6) of Example 1 is combined with a resin primer. The photothermal composite anti-icing coating is constructed on the surface of a glass substrate by first spraying the primer and then spraying the super-hydrophobic CuS@SiO2 composite material. The coating is compared with a glass sheet coating sample coated only with a super-hydrophobic SiO2 coating to explore the deicing effect of the obtained CuS@SiO2 photothermal composite anti-icing coating. The specific steps include:
[0106] (1) Under magnetic stirring conditions, 9 g of hydroxy acrylic resin FX-9024, 1.5 g of fluorocarbon resin, 4 g of alkyd resin, 1.2 g of PP polypropylene resin, 0.3 mL of KH550 solution (KH550: H2O = 0.12 mL: 0.18 mL), and 2 g of nylon powder were added to 30 mL of butyl acetate in sequence, and stirred for 24 h to obtain a resin primer;
[0107] (2) On the surface of the glass substrate, first spray the resin primer obtained in step 1), then spray the super-hydrophobic CuS@SiO2 photothermal composite coating described in Example 1, and dry them to obtain the super-hydrophobic CuS@SiO2 photothermal anti-icing coating.
[0108] The specific test steps are as follows:
[0109] a) Comparison of the delayed freezing time of CuS@SiO2 photothermal composite anti-icing coating and super-hydrophobic SiO2 coating under the same light intensity and different temperatures: two glass sheets were placed on a condensation table at the same ambient temperature. When the surface temperature of the glass sheet stabilized to the same as the ambient temperature, an equal amount of methyl blue dye droplets were added, and then a xenon lamp was turned on to irradiate the coating surface and time was kept, and the complete freezing time of the droplets was recorded;
[0110] b) Comparison of the delayed freezing time of the CuS@SiO2 photothermal composite anti-icing coating and the superhydrophobic SiO2 coating at the same temperature and different light intensities, using the same method as above.
[0111] c) Compare the ice melting effects of the above two coatings under the same light: Use a cylindrical mold to drop the same amount of water on the surface of the above two glass pieces and place them on a condensation table for 6 hours to ensure that the two glass pieces are adhered with icicles of the same shape and volume, and ensure that the glass pieces and the condensation table are inclined at 30°. When the surface temperature of the two glass pieces stabilizes to the same temperature as the ambient temperature, turn on the xenon lamp and increase the light intensity to 1kW / m 2 Then start irradiation and timing, and record the time it takes for the icicle to slide.
[0112] d) Test of the wear resistance of CuS@SiO2 photothermal composite anti-icing coating: A 10 cm × 10 cm × 0.5 mm anti-icing coating glass slide was placed under a load of 1000 g at a constant slow speed (about 1 cm s -1 ) was moved on sandpaper (800 mesh) with a reciprocating motion of 10 cm per cycle, and 20 cm was recorded as one abrasion cycle. After 500 abrasion cycles, the contact angle of the sample was tested.
[0113] Fig.10 The morphology of the obtained CuS@SiO2 photothermal composite anti-icing coating sample and superhydrophobic SiO2 coating; the area of the glass sheet is 10×5cm.
[0114] Fig.11The scanning electron microscope (SEM) image of the anti-icing coating sample obtained in this application example represents that the coating has a micro-nano hierarchical structure: the super-hydrophobic CuS@SiO2 coating obtained by the present invention is deposited on the surface of the resin primer, and the surface of the super-hydrophobic coating obtained shows micron-scale papillary composite deposits, and the particle size of the micron-scale papillary composite deposits is approximately between 70 and 100 μm (as shown in Figures a and b), mainly composed of CuS@SiO2 composite nanoparticles and nano-scale SiO2 particles. The present invention combines the surface modification of low surface energy materials with micro-nano structures and other means, and the constructed micro-nano rough structure makes the CuS@SiO2 anti-icing coating have excellent super-hydrophobicity and wear and weather resistance.
[0115] Fig.12 The CuS@SiO2 photothermal composite anti-icing coating sample and the ordinary super-hydrophobic SiO2 coating sample were compared at 0.5kW / m 2 , Comparison of delayed freezing time at different temperatures. As the ambient temperature decreases, the difference in delayed freezing time between the super-hydrophobic CuS@SiO2 coating sample and the ordinary super-hydrophobic SiO2 coating sample becomes larger. For example, at -20°C, the delayed freezing time of the CuS@SiO2 coating sample is 1.96 times that of the ordinary super-hydrophobic SiO2 coating sample; when the temperature drops to -15°C, the CuS@SiO2 coating sample does not even freeze within 30 minutes, while the ordinary super-hydrophobic SiO2 coating sample is completely frozen in 17 minutes.
[0116] Fig.13 The comparison chart of the delayed freezing time of the obtained CuS@SiO2 photothermal composite anti-icing coating sample and the ordinary super-hydrophobic SiO2 coating sample at -20℃ and different light intensity is shown in the figure. As can be seen from the figure, the freezing time of the ordinary super-hydrophobic SiO2 coating sample does not change much under different light intensities, while the freezing time of the CuS@SiO2 anti-icing coating sample is significantly prolonged as the light intensity increases, even at 1kW / m 2 Under the condition of low temperature, the droplets on the surface of the CuS@SiO2 anti-icing coating sample did not freeze within 30 minutes, while the super-hydrophobic SiO2 coating sample completely froze in about 5 minutes, which confirmed the excellent anti-icing performance of the sample.
[0117] Fig.14 Comparison of CuS@SiO2 photothermal composite anti-icing coating sample and common super-hydrophobic SiO2 coating sample at -20℃ and 1kW / m 2The morphology comparison diagram of the ice melting process under light intensities of different intensity. Within 30 minutes, the icicles on the surface of the ordinary superhydrophobic SiO2 coating sample hardly changed, while the icicles on the surface of the CuS@SiO2 anti-icing coating sample gradually melted into water droplets at the contact point between the bottom of the icicles and the coating surface as the illumination time prolonged. Then, after 30 minutes, the icicles slipped and then detached from the CuS@SiO2 coating surface and slid onto the condensation table. However, the icicles on the surface of the ordinary superhydrophobic SiO2 coating sample still did not detach from the coating surface after 1 hour. The comparison of the time it took for the icicles to detach from the two coating surfaces confirmed the deicing performance of the CuS@SiO2 anti-icing coating sample.
[0118] Fig.15 The following is a comparison of the wear resistance test results of the anti-icing coating samples obtained in this application example. The left picture shows the surface morphology and contact angle of the coating before the test, and the right picture shows the surface morphology and contact angle of the coating after the test. The CuS@SiO2 photothermal anti-icing coating with a size of 2.5cm×2.5cm×0.8mm (under a load of 100g, 1600Pa) was heated at a constant slow speed (about 1cm·s -1 ) is moved horizontally on sandpaper (800 mesh) for 20 cm to complete a wear cycle. After 500 wear cycles, obvious scratches have appeared on the coating surface, but the contact angle can still reach 150°, and the anti-icing coating has good wear resistance.
[0119] Application Example 2
[0120] The super-hydrophobic CuS@SiO2 composite photothermal coating of the present invention is applied to prepare water evaporation materials, and a CuS@SiO2 photothermal water evaporation material with a super-hydrophobic / super-hydrophilic Janus structure is constructed and applied to the field of water evaporation + photocatalysis; specifically as follows:
[0121] A NaCl-MB dye solution with a sodium chloride concentration of 3.5wt% and a methylene blue concentration of 5mg / L was prepared to simulate seawater. The CuS@SiO2 photothermal water evaporator with the Janus structure obtained in Example 3 was placed in a beaker filled with 50mL of the NaCl-MB dye solution. The beaker was then placed in a dark environment for 30min to achieve adsorption-desorption equilibrium. The beaker was then placed on a balance and a xenon lamp of model CEL-S500-T5 was used at 1kW / m 2 The beaker was irradiated with light at a low intensity. The mass loss of the dye solution was recorded every 10 minutes. In addition, 3 mL of the dye solution was taken from the beaker with a pipette every 20 minutes, and the absorbance change of the dye solution was stored and tested. Since CuS micro-nanoparticles easily generate electrons and holes, and easily react with H2O2 to promote degradation, 0.5 mL of H2O2 (30 m%) was added to 50 mL of methyl blue dye solution to promote degradation.
[0122] Fig.16Comparison photos of the Janus structure CuS@SiO2 water evaporator described in this application example 3 before and after being placed in the NaCl-MB dye solution for 90 minutes. It can be seen that the lower surface of the evaporator has good superhydrophilicity and will be immersed in the dye solution so as to adsorb dye molecules and facilitate the degradation of the dye solution. The upper surface has good superhydrophobic properties and thus floats on the liquid surface, ensuring that the evaporator can receive light at a close distance to maximize the photocatalytic degradation effect. In addition, after 90 minutes, the color of the dye solution changes from blue to colorless, indicating that most of the methyl blue molecules in the dye solution have been degraded into small molecular organic matter such as H2O and CO2, and the dye solution gradually becomes pure salt water.
[0123] Fig.17 The figure shows the evaporation efficiency of the above-mentioned Janus structure CuS@SiO2 water evaporator evaporating NaCl-MB dye solution. It can be seen from the figure that within 2 hours, the evaporation efficiency of the dye solution by "MF" (i.e., pure foam without CuS@SiO2 composite material) is much lower than the evaporation efficiency of the Janus structure CuS@SiO2 water evaporator. Fig.15 The slope of the curve gives the evaporation efficiency of "MF" as 0.534 kg / m 2 / h, while the evaporation efficiency of the Janus structure CuS@SiO2 water evaporator is 2.148kg / m 2 / h, the efficiency is 4.02 times that of the former. It can be seen that the Janus structure CuS@SiO2 water evaporator has excellent photothermal evaporation of water, and the CuS@SiO2 nanocomposite material provides an effective way for solar-driven seawater desalination.
[0124] Fig.18 The absorbance curve of the above NaCl-MB dye solution within 120 minutes of evaporation time. It can be seen from the figure that after 120 minutes, the absorbance of the pure dye solution containing only "MF" only decreased slightly; while the absorbance of the dye solution containing the Janus structure CuS@SiO2 water evaporator decreased significantly within 90 minutes. According to calculations, within one hour, the degradation rate of the dye solution containing only "MF" was 21%, while the degradation rate of the dye solution containing the Janus structure CuS@SiO2 water evaporator was 91%, which is 4.3 times that of the former. It can be seen that the Janus structure CuS@SiO2 water evaporator also has an excellent photocatalytic degradation effect on the dye solution.
[0125] Comparative Example 1
[0126] A CuS@SiO2 photothermal composite dispersion, the preparation method of which comprises the following steps:
[0127] 1) Under stirring conditions, 1.5 mL of NaOH solution (1.8 mol / L) and 5 mL of tetraethyl orthosilicate (TEOS) were added to 25 mL of ethanol in sequence, and the mixture was hydrolyzed for 24 h under stirring conditions to obtain a super-hydrophilic SiO2 dispersion system;
[0128] 2) adding 5 mL of hexamethyldisilazane (HMDS) to the dispersion system obtained in step (1), and continuing stirring for 8 h to obtain a super-hydrophobic SiO2 dispersion;
[0129] 3) Weigh 0.256 g sulfur powder (8 mmol) into a 50 mL three-necked flask, add 40 mL octadecene (ODE) and 10 mL oleylamine (OM) in sequence, and heat to 90 °C at a rate of 10 °C / min under vacuum conditions, and keep at this temperature for 30 min to obtain an orange-red transparent S precursor solution;
[0130] 4) Ar gas was introduced and the obtained S precursor solution was cooled to room temperature, and then 0.799 g of copper acetate monohydrate Cu(Ac)2·H2O (4 mmol) was added, and vacuum was applied at room temperature for 30 min, and then the temperature was raised to 200°C at a rate of 10°C / min, and kept at this temperature for 30 min to obtain a black-green dispersion; the mixture was further cooled to room temperature under Ar atmosphere to obtain a CuS black-green dispersion (concentration of 0.008 M);
[0131] 5) washing the CuS dispersion obtained in step 2) twice with methanol as a detergent by centrifuging (4000 rpm, 5 min) to separate the nanocrystal precipitate, and then adding toluene to evenly disperse the precipitate to obtain a CuS-toluene dispersion, wherein the solid-liquid ratio of the CuS nanocrystal precipitate to toluene is 0.13 g / mL;
[0132] 6) Add 6 mL of the CuS-toluene dispersion obtained in step 5) to the super-hydrophobic SiO2 dispersion obtained in step 1), and stir and mix for 4 hours to obtain a super-hydrophilic CuS@SiO2 photothermal composite dispersion.
[0133] 7) Add 6 mL of the CuS-toluene dispersion obtained in step 5) to the super-hydrophobic SiO2 dispersion obtained in step 2), and stir and mix for 4 hours to obtain a super-hydrophobic CuS@SiO2 photothermal composite dispersion.
[0134] Comparative Example 2
[0135] A CuS@SiO2 photothermal composite dispersion, the preparation method of which comprises the following steps:
[0136] 1) Under magnetic stirring conditions, weigh 0.78 g of commercially available high-purity CuS particles (particle size 50-100 nm, purity 99.9%), slowly pour into 25 mL of ethanol and stir for 30 min to make it evenly dispersed;
[0137] 2) adding 1.5 mL of NaOH solution (1.8 mol / L) and 5 mL of tetraethyl orthosilicate to the solution obtained in step 1) in sequence, and performing a hydrolysis reaction under stirring for 24 h to obtain a super-hydrophilic CuS@SiO2 photothermal composite dispersion;
[0138] 3) Add 5.0 mL of hexamethyldisilazane (HMDS) to the solution system in step 2) and continue stirring for 12 hours to obtain a super-hydrophobic CuS@SiO2 photothermal composite dispersion.
[0139] The super-wettable CuS@SiO2 photothermal composite dispersion obtained in the above-mentioned comparative examples 1 and 2 was used to prepare a CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure. The specific preparation method includes: preparing melamine foam (abbreviated as MF) and cutting it into squares (area 2.5×2.5 cm 2 , thickness is 0.5 cm), and 1 mL of superhydrophobic CuS@SiO2 photothermal composite material is sprayed on the upper surface of MF, and 2.5 mL of superhydrophilic CuS@SiO2 material is taken and the lower surface of MF is immersed therein to make it fully absorbed, and then dried to obtain the superhydrophobic / superhydrophilic Janus structure CuS@SiO2 photothermal water evaporator.
[0140] The super-hydrophobic CuS@SiO2 photothermal composite dispersion obtained in the above-mentioned comparative examples 1 and 2 is used to prepare a photothermal composite anti-icing coating. The specific preparation method includes: 1) Under stirring conditions, hydroxy acrylic resin, fluorocarbon resin, alkyd resin, polypropylene resin, silane coupling agent, and filler are added to an organic solvent (butyl acetate, etc.) in sequence, and stirred (12 to 24 hours to obtain a resin primer); 2) On the surface of a glass substrate (7.5×2.5 cm), first spray the resin primer obtained in step 1) as a binder to improve the wear and weather resistance of the coating, and then when the primer reaches surface dry, spray the super-hydrophobic CuS@SiO2 photothermal composite coating, and dry to obtain a super-hydrophobic CuS@SiO2 photothermal anti-icing coating.
[0141] Comparative Example 3
[0142] A CuS@SiO2 photothermal composite dispersion, the preparation method of which comprises the following steps:
[0143] 1) Weigh 0.256 g sulfur powder (8 mmol) into a 50 mL three-necked flask, add 40 mL octadecene (ODE) and 10 mL oleylamine (OM) in sequence, and heat to 90 °C at a rate of 10 °C / min under vacuum conditions, and keep at this temperature for 30 min to obtain an orange-red transparent S precursor solution;
[0144] 2) Ar gas was introduced and the obtained S precursor solution was cooled to room temperature, and then 0.799 g of copper acetate monohydrate Cu(Ac)2·H2O (4 mmol) was added, and vacuum was applied at room temperature for 30 min, and then the temperature was raised to 200°C at a rate of 10°C / min, and kept at this temperature for 30 min to obtain a black-green dispersion; the mixture was further cooled to room temperature under Ar atmosphere to obtain a CuS black-green dispersion (concentration of 0.008 M);
[0145] 3) washing the CuS dispersion obtained in step 2) twice with methanol as a detergent by centrifuging (4000 rpm, 5 min) to separate the nanocrystal precipitate, and then adding toluene to evenly disperse the precipitate to obtain a CuS-toluene dispersion, wherein the solid-liquid ratio of the CuS nanocrystal precipitate to toluene is 0.13 g / mL;
[0146] 4) Under magnetic stirring, take 6 mL of the CuS-toluene dispersion obtained in step 3), slowly pour it into 25 mL of ethanol and stir for 30 min to make it evenly dispersed and evaporate the toluene;
[0147] 5) 1.5 mL of NaOH solution (1.8 mol / L) and 5 mL of tetramethyl orthosilicate were added to the mixed solution obtained in step 4) in sequence, and the mixture was hydrolyzed for 24 h under stirring to obtain a super-hydrophilic CuS@SiO2 photothermal composite coating;
[0148] 6) Add 5.0 mL of hexamethyldisilazane (HMDS) to the solution system in step 5) and continue stirring for 12 hours to obtain a hydrophobic CuS@SiO2 photothermal composite coating;
[0149] The CuS@SiO2 dispersion of Comparative Example 3 was used to prepare a Janus structure CuS@SiO2 water evaporator. The specific steps included: preparing melamine foam (abbreviated as MF) and cutting it into squares (area 2.5×2.5 cm 2 , thickness is 0.5cm), and 1mL of the hydrophobic CuS@SiO2 photothermal composite material obtained in step 6) is sprayed on the upper surface of MF, and 2.5mL of the superhydrophilic CuS@SiO2 material obtained in step 5) is taken and the lower surface of MF is immersed therein to make it fully absorbed, and then dried to obtain a CuS@SiO2 photothermal water evaporator with a Janus structure.
[0150] The hydrophobic CuS@SiO2 photothermal composite material obtained in the above comparative example 3 is used to prepare a hydrophobic CuS@SiO2 photothermal coating. The specific steps include: 1) Under stirring conditions, hydroxy acrylic resin, fluorocarbon resin, alkyd resin, polypropylene resin, silane coupling agent, and filler are added to an organic solvent (butyl acetate, etc.) in sequence, and stirred (12 to 24 hours to obtain a resin primer); 2) On the surface of a glass substrate (7.5×2.5 cm), the resin primer obtained in step 1) is first sprayed as a binder to improve the wear and weather resistance of the coating, and then when the primer reaches surface dry, the hydrophobic CuS@SiO2 photothermal composite coating is sprayed, and dried to obtain a hydrophobic CuS@SiO2 photothermal anti-icing coating.
[0151] The performance test results of the photothermal water evaporator and the photothermal anti-icing coating prepared in Example 1 and Comparative Examples 1 to 3 are shown in Table 1.
[0152] Table 1 Performance test results of water evaporators and anti-icing coatings prepared in Example 1 and Comparative Examples 1 to 3
[0153]
[0154]
[0155] By comparing the above table, it can be seen that the super-wettable CuS@SiO2 photothermal composite material obtained by the present invention has excellent super-hydrophobicity and photothermal conversion performance. Since the typical microscopic morphology of the CuS@SiO2 photothermal composite material prepared by the present invention is that SiO2 in situ coats the flaky CuS nanocrystalline phase to grow to obtain a core-shell structure, after being modified by a low surface energy material, it is combined with a resin-based primer to construct a special micro-nano rough structure, which makes the CuS@SiO2 anti-icing coating have excellent super-hydrophobicity and wear resistance and weather resistance. The CuS@SiO2 photothermal composite anti-icing coating of the present invention can effectively capture air to reduce the actual contact area between water droplets and the substrate, enhance its super-hydrophobic performance, and significantly delay the freezing time due to its special micro-nano structure and effective low surface energy modification; the Janus structure CuS@SiO2 photothermal water evaporator not only has good self-floating properties, but also can efficiently capture sunlight and continuously reflect it in the micro-nano porous structure to improve the absorption of sunlight, thereby giving full play to the photothermal conversion effect to increase the surface temperature, enhance the water evaporation rate of the evaporator and the photocatalytic degradation efficiency of the dye solution.
[0156] Comparative Example 4
[0157] A super-hydrophobic CuS@SiO2 photothermal composite anti-icing coating, the specific preparation steps include:
[0158] (1) Under magnetic stirring conditions, 6 g of alkyd resin, 1.8 g of PP polypropylene resin, 1 g of fluorocarbon resin, 0.6 mL of KH550 solution (KH550: H2O = 0.24 mL: 0.36 mL), and 2 g of nylon powder were added to 30 mL of butyl acetate in sequence, and stirred for 24 h to obtain a resin primer;
[0159] (2) Preparation of super-hydrophobic CuS@SiO2 photothermal composite coating, see Example 1;
[0160] (3) On the surface of the glass substrate, first spray the resin primer obtained in step (1), then spray the super-hydrophobic CuS@SiO2 photothermal composite coating described in Example 1, and dry them to obtain a super-hydrophobic CuS@SiO2 photothermal anti-icing coating.
[0161] The super-hydrophobic CuS@SiO2 photothermal composite anti-icing coating obtained in Comparative Example 4 was compared with the super-hydrophobic CuS@SiO2 photothermal composite anti-icing coating described in Application Example 1 to test the wear resistance of the two coatings. The specific steps are as follows:
[0162] Two CuS@SiO2 photothermal anti-icing coatings of the same size (2.5 cm × 2.5 cm × 0.8 mm) were heated at a constant slow speed (about 1 cm·s -1 ) is moved horizontally on sandpaper (800 mesh) for 20 cm to complete one abrasion cycle. The contact angle of the sample is measured every 100 abrasion cycles.
[0163] Finally, it was measured that the contact angle of the super-hydrophobic CuS@SiO2 photothermal composite anti-icing coating obtained in Comparative Example 4 after 300 wear cycles was 144°, while the contact angle of the super-hydrophobic CuS@SiO2 photothermal composite anti-icing coating described in Application Example 1 after 500 wear cycles was 150°, and the coating still maintained super-phobicity.
[0164] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
Claims
1. A method for preparing a super-wettable CuS@SiO2 photothermal composite material, characterized in that: The steps include: (1) sulfur powder, octadecene, and oleylamine are sequentially added to a reaction vessel, and a first heating reaction is performed under vacuum conditions to obtain an orange-red transparent S precursor solution; (2) Cool the S precursor solution to room temperature by passing a protective atmosphere, then add copper salt, conduct a second heating reaction under vacuum conditions, and then cool to room temperature by passing a protective atmosphere to obtain a black-green CuS dispersion. (3) The CuS dispersion obtained in step (2) is subjected to centrifugal separation using alcohol solvent I as a detergent to obtain a nanocrystal precipitate; and then toluene is added to uniformly disperse the precipitate to obtain a CuS-toluene dispersion; (4) adding the CuS-toluene dispersion obtained in step (3) to the alcohol solvent II under magnetic stirring conditions, stirring the dispersion to uniformly disperse the dispersion and volatilize the toluene; (5) adding an alkali solution and a hydrolyzable silicon source to the dispersion obtained in step (4) in sequence, and continuing to react by stirring to obtain a super-hydrophilic CuS@SiO2 photothermal composite material; (6) Adding a silane-based low surface energy material to the reaction system obtained in step (5), continuing the stirring reaction, and obtaining a super-hydrophobic CuS@SiO2 photothermal composite material.
2. The preparation method according to claim 1, characterized in that: The hydrolyzable silicon source is one or more of tetraethyl orthosilicate and tetrabutyl orthosilicate.
3. The preparation method according to claim 1, characterized in that: The silane-based low surface energy substance is one or more of hexamethyldisilazane, methyltriethoxysilane, and hexadecyltrimethoxysilane.
4. The preparation method according to claim 1, characterized in that: The temperature used in step (1) of the first heating reaction is 90-100°C and the time is 20-40 minutes; the temperature used in step (2) of the second heating reaction is 150-220°C and the time is 20-40 minutes.
5. The preparation method according to claim 1, characterized in that: In the CuS-toluene dispersion, the concentration of CuS is (0.10-0.15) g / mL.
6. The preparation method according to claim 1, characterized in that: The volume ratio of the CuS-toluene dispersion, alcohol solvent II, alkali solution, hydrolyzable silicon source, and silane-based low surface energy material in steps (4) to (6) is (1 to 5): (5 to 7): (0.2 to 0.4): (1 to 1.4): (0.6 to 1).
7. The preparation method according to claim 1, characterized in that: The stirring treatment time of step (4) is 0.5 to 1 h; the stirring reaction time of step (5) is 20 to 24 h; and the stirring reaction time of step (6) is 6 to 12 h.
8. The super-wettable CuS@SiO2 photothermal composite material prepared by the preparation method according to any one of claims 1 to 7.
9. A CuS@SiO2 photothermal water evaporator with a super-hydrophobic / super-hydrophilic Janus structure prepared using the super-wettable CuS@SiO2 photothermal composite material according to claim 1.
10. A photothermal composite anti-icing coating prepared using the super-wettable CuS@SiO2 photothermal composite material according to claim 1.
Citation Information
Patent Citations
Method for preparing fluorescence medicine carrying photo-thermal multifunctional CuS nanodisk aggregate composite nanocapsule
CN105687160A
Copper sulfide / silicon dioxide / manganese dioxide nano composite particle, preparation method and application
CN111202720A
Cited By
Solar photo-thermal interface evaporation coating and preparation method thereof
CN119410218A
MXene-based deicing super-hydrophobic paint, coating, preparation method and application of coating
CN120137488A
A mxene-based deicing superhydrophobic coating, coating and preparation method and coating application
CN120137488B
Multi-layer carbon fiber composite material with anti-icing function and preparation method thereof
CN120269850A