Magnetic plastic marine composite anticorrosive material and preparation method thereof
By combining ferromagnetic materials with polyethylene wax, a magnetic plastic marine composite anti-corrosion material is formed, which solves the anti-corrosion problem of small-angle steel components in the marine environment and achieves efficient anti-corrosion protection for offshore steel components. The corrosion degree reaches A level and overcomes the problem. The problem of spray material not reaching the bottom layer.
Patent Information
- Application Number
- CN202411053690.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult for the existing technology to effectively protect steel components with an angle less than 60 degrees in the marine environment. The anti-corrosion materials sprayed cannot reach the bottom layer of the component, resulting in the corrosion that cannot be completely resolved. Moreover, conventional protection technology cannot solve the anti-corrosion problem of steel components with small angles.
By adding ferromagnetic materials to melted polyethylene wax to form a matrix layer material, and spraying it on the surface of steel components, combined with low-density polyethylene as a protective layer material, a tight magnetic plastic marine composite anti-corrosion material is formed, using magnetic materials and steel The components form a tight combination, and are directionally adsorbed and sprayed to form a matrix layer to improve the protective effect.
It has achieved close integration and good anti-corrosion performance for offshore steel components, with the corrosion grade reaching Grade A, overcoming the anti-corrosion problem of small-angle steel components, and improving the anti-falling performance of protective materials.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion materials, and in particular relates to a magnetic plastic marine composite anti-corrosion material and a preparation method thereof. Background Art
[0002] In the process of marine development, the corrosion of metal parts has always been a problem. Large marine cargo ships, heavy ships and offshore shoreline facilities, including pipeline corridors, offshore farms, cargo ships, reefs and houses of large facilities, usually have a part extending into the sea water, or extending into the mud and sand at the bottom of the sea water, or a part passing through the rock and another part exposed in the sea water. Some of these parts have angle steel angles less than 60 degrees, which cannot be reached by the current protection technology operator's arm, nor can manual grinding wheel equipment.
[0003] According to the National Association of Corrosion Engineers of the United States, the economic losses caused by metal corrosion in the world each year are as high as 4 trillion US dollars, accounting for about 3.6% of the global GDP. Using appropriate protection strategies, it is conservatively estimated that the economic losses can be reduced by about 15% to 35%. The indirect economic losses caused by metal corrosion should not be ignored, such as the time cost of disassembly of components, replacement and maintenance of equipment, and treatment of environmental pollution caused by metal corrosion, which are difficult to accurately assess. In addition, metal structures in marine environments are expensive assets completed under more unfavorable conditions. The consequences of metal corrosion in marine environments are often more difficult to deal with than corrosion in atmospheric environments. In summary, in harsh marine environments, metal corrosion will not only cause huge economic losses, but even human life safety cannot be effectively guaranteed. It is an issue that needs to be considered and solved in the development of marine equipment. Therefore, researchers have been looking for practical and economical strategies to improve the corrosion resistance of metals and extend the service life of metals, such as electrochemical protection, corrosion inhibitors, anti-corrosion coatings, and material structure optimization.
[0004] Patent CN108178981A discloses an anti-corrosion material for an offshore platform. The invention uses sodium dodecyl sulfate as a surfactant to prepare a pyrrole aqueous solution. The constant current method is used in 1Cr l8 A conductive polypyrrole film layer is polymerized on the surface of N i9T i stainless steel. The corrosion test of this anti-corrosion material in 0.3 mol / L HCl aqueous solution found that the anti-corrosion material layer of the offshore platform can effectively inhibit the active corrosion of stainless steel, significantly improve its pitting potential, and the protective effect of the film layer on the substrate increases with the increase of the film layer thickness.
[0005] Patent CN116239905B discloses a method for preparing a multi-effect marine anti-corrosion and anti-fouling coating material. The invention first prepares a silicon dioxide protective layer for synthesized cuprous oxide nanoparticles. When the pH value of the reaction solution is lower than the pKa of the aniline molecule, an aniline solution is added to the system, and the aniline adheres to the surface of the silicon dioxide particles. Finally, the polyaniline shell is wrapped around the silicon dioxide protective layer by an in-situ oxidative polymerization method to obtain a cuprous oxide / silicon dioxide / polyaniline core-shell material. In the prepared coating material, polyaniline is uniformly dispersed in the coating, which not only reduces coating defects, but also promotes the formation of a uniform and complete passivation film of polyaniline on the metal surface, thereby improving the anti-corrosion effect of the coating.
[0006] Anti-corrosion materials need to be tightly combined with steel components to achieve anti-corrosion effects. If the coating cannot be tightly combined, the protection work cannot be thoroughly implemented. In the existing technology, the anti-corrosion problem of small-angle difficult components in in-service offshore steel structures is a technical problem that all technologies are reluctant to touch but cannot be avoided. The sprayed anti-corrosion material cannot reach the bottom layer of the component, so that the rust of the bottom layer cannot be completely solved, and bubbling and arching of the coating will occur in the later stage. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention solves the problems raised in the background art by constructing a plastic marine composite anticorrosive material with magnetic function. Specifically, the technical solution of the present invention includes the following contents:
[0008] One of the purposes of the present invention is to provide a method for preparing a magnetic plastic marine composite anticorrosive material, the preparation method comprising the following steps:
[0009] S1: adding the ferromagnetic material into the molten polyethylene wax and mixing and stirring at a speed of 200 r / min to 400 r / min for 20 min to 30 min, and cooling and granulating after the stirring to obtain the matrix layer material;
[0010] S2: low-density polyethylene LDPE with a number average molecular weight of 14000-18000, a particle size of 60 μm-100 μm, and a drop melting point of 160°C-220°C is used as the protective layer material;
[0011] S3: spraying the matrix layer material on the surface of the steel component, and then spraying the protective layer material on the surface of the matrix layer material on the steel component for curing to obtain the magnetic plastic marine composite anti-corrosion material.
[0012] Furthermore, the diameter of the ferromagnetic material is 10 μm to 20 μm.
[0013] Furthermore, the ferromagnetic material is ferrite, neodymium iron boron or iron cobalt nickel.
[0014] Furthermore, the number average molecular weight of the polyethylene wax is 8000-12000, and the drop melting point of the polyethylene wax is 120°C-140°C.
[0015] Furthermore, the melting temperature of the melted polyethylene wax is 120°C to 140°C.
[0016] Furthermore, the added amount of the ferromagnetic material is 0.1% to 0.5% of the mass of the polyethylene wax.
[0017] Furthermore, the container for mixing and stirring the ferromagnetic material and the molten polyethylene wax includes an aluminum container or a copper container.
[0018] Furthermore, the thickness of the matrix layer material sprayed on the surface of the steel component is 0.2 mm to 0.4 mm.
[0019] Furthermore, the mass ratio of the polyethylene wax to the low-density polyethylene LDPE is 1:3.
[0020] Furthermore, the low-density polyethylene LDPE can be prepared from natural latex, natural rubber or oligoisoprene, and needs to be vulcanized on site.
[0021] Preferably, the drop melting point of the low-density polyethylene LDPE is 160°C to 180°C.
[0022] The second object of the present invention is to provide a magnetic plastic marine composite anti-corrosion material prepared by the method for preparing the magnetic plastic marine composite anti-corrosion material.
[0023] Furthermore, the application environment of the magnetic plastic marine composite anti-corrosion material includes a salt spray corrosion environment.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention creatively combines ferromagnetic material into polyethylene wax, modifies the polyethylene wax to obtain a matrix layer material, and sprays the protective layer material onto the matrix layer material, thereby forming a magnetic plastic marine composite anti-corrosion material that is tightly bonded with the matrix layer material. The ferromagnetic material can form magnetic adsorption with offshore steel components, thereby improving the tight bonding between the protective material and the offshore steel components, and the magnetic material can guide the polyethylene wax to be directional-adsorbed and sprayed on the surface of the difficult steel components and form a matrix layer, thereby overcoming the technical difficulty that the current conventional technology cannot solve the anti-corrosion of small-angle steel components, and improving the anti-corrosion performance of offshore steel components.
[0026] (2) According to the experimental results of Examples 1 to 5, it can be seen that the magnetic plastic marine composite anti-corrosion material of the present invention is tightly combined with the steel components, and the rust grade reaches Class A, indicating that the magnetic plastic marine composite anti-corrosion material of the present invention has good anti-corrosion and anti-falling properties, and can achieve the anti-corrosion protection function for offshore steel components. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly and completely described below through the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0028] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.
[0029] Embodiment 1:
[0030] A method for preparing a magnetic plastic marine composite anticorrosive material, specifically comprising the following steps:
[0031] S1: Weigh 1 kg of polyethylene wax with a number average molecular weight of 8000 and a drop melting point of 120°C, place it in an aluminum container and heat it to 120°C to make the polyethylene wax in a molten state, then add 10 g of ferrite with a diameter of 10 μm into the molten polyethylene wax, stir and mix at a speed of 400 r / min for 20 minutes, cool to room temperature after stirring, and then granulate to obtain a matrix layer material;
[0032] S2: Take 3 kg of low-density polyethylene LDPE with a number average molecular weight of 14,000, a particle size of 60 μm, and a drop melting point of 160° C. as the protective layer material;
[0033] S3: The matrix layer material obtained in S1 is first sprayed on the surface of the steel component, and the spraying thickness is controlled to be 0.2 mm. Then the protective layer material in S2 is sprayed on the matrix layer material on the surface of the steel component. After complete solidification, the magnetic plastic marine composite anti-corrosion material is obtained.
[0034] Embodiment 2:
[0035] A method for preparing a magnetic plastic marine composite anticorrosive material, specifically comprising the following steps:
[0036] S1: 1 kg of polyethylene wax with a number average molecular weight of 9000 and a melting point of 130°C is weighed and placed in an aluminum container and heated to 125°C to melt the polyethylene wax, then 20 g of ferrite with a diameter of 12 μm is added to the melted polyethylene wax, and the mixture is stirred at a speed of 300 r / min for 22 min. After the stirring is completed, the mixture is cooled to room temperature, and then granulated to obtain a matrix layer material;
[0037] S2: Take 3 kg of low-density polyethylene LDPE with a number average molecular weight of 15,000, a particle size of 70 μm, and a drop melting point of 180°C as the protective layer material;
[0038] S3: The matrix layer material obtained in S1 is first sprayed on the surface of the steel component, and the spraying thickness is controlled to be 0.2 mm. Then the protective layer material in S2 is sprayed on the matrix layer material on the surface of the steel component. After complete solidification, the magnetic plastic marine composite anti-corrosion material is obtained.
[0039] Embodiment 3:
[0040] A method for preparing a magnetic plastic marine composite anticorrosive material, specifically comprising the following steps:
[0041] S1: Weigh 1 kg of polyethylene wax with a number average molecular weight of 10,000 and a drop melting point of 150°C, place it in a copper container and heat it to 130°C to make the polyethylene wax in a molten state, then add 30 g of ferrite with a diameter of 14 μm into the molten polyethylene wax, stir and mix at a speed of 200 r / min for 24 minutes, cool to room temperature after stirring, and then granulate to obtain a matrix layer material;
[0042] S2: Take 3 kg of low-density polyethylene LDPE with a number average molecular weight of 16,000, a particle size of 80 μm, and a drop melting point of 200°C as the protective layer material;
[0043] S3: The matrix layer material obtained in S1 is first sprayed on the surface of the steel component, and the spraying thickness is controlled to be 0.3 mm. Then the protective layer material in S2 is sprayed on the matrix layer material on the surface of the steel component. After complete solidification, the magnetic plastic marine composite anti-corrosion material is obtained.
[0044] Embodiment 4:
[0045] A method for preparing a magnetic plastic marine composite anticorrosive material, specifically comprising the following steps:
[0046] S1: Weigh 1 kg of polyethylene wax with a number average molecular weight of 11000 and a melting point of 155°C, place it in a copper container and heat it to 135°C to make the polyethylene wax molten, then add 10 g of NdFeB with a diameter of 16 μm into the molten polyethylene wax, stir and mix at a speed of 200 r / min for 26 minutes, cool to room temperature after stirring, and then granulate to obtain a matrix layer material;
[0047] S2: Take 3 kg of low-density polyethylene LDPE with a number average molecular weight of 17000, a particle size of 90 μm, and a drop melting point of 220°C as the protective layer material;
[0048] S3: The matrix layer material obtained in S1 is first sprayed on the surface of the steel component, and the spraying thickness is controlled to be 0.3 mm. Then the protective layer material in S2 is sprayed on the matrix layer material on the surface of the steel component. After complete solidification, the magnetic plastic marine composite anti-corrosion material is obtained.
[0049] Embodiment 5:
[0050] A method for preparing a magnetic plastic marine composite anticorrosive material, specifically comprising the following steps:
[0051] S1: Weigh 1 kg of polyethylene wax with a number average molecular weight of 12000 and a drop melting point of 140°C, place it in a copper container and heat it to 140°C to make the polyethylene wax in a molten state, then add 10 g of iron, cobalt and nickel with a diameter of 20 μm into the molten polyethylene wax, stir and mix at a speed of 200 r / min for 30 minutes, cool to room temperature after stirring, and then granulate to obtain a matrix layer material;
[0052] S2: Take 3 kg of low-density polyethylene LDPE with a number average molecular weight of 18,000, a particle size of 100 μm, and a drop melting point of 180°C as the protective layer material;
[0053] S3: The matrix layer material obtained in S1 is first sprayed on the surface of the steel component, and the spraying thickness is controlled to be 0.4 mm. Then the protective layer material in S2 is sprayed on the matrix layer material on the surface of the steel component. After complete solidification, the magnetic plastic marine composite anti-corrosion material is obtained.
[0054] The steel components used for spraying in Examples 1 to 5 are clean steel components with an angle steel angle of less than 60°. The surface of the steel components needs to meet the following standard requirements, which are: 1. "Surface treatment of steel before coating - Visual assessment of surface cleanliness - Part 1: Rust grade and treatment grade of uncoated steel surfaces and steel surfaces after complete removal of original coatings" GB / T 8923.1-2011; 2. "Surface treatment of steel before coating - Visual assessment of surface cleanliness - Part 2: Treatment grade of coated steel surfaces after partial removal of original coatings" GB / T 8923.2-2008. The spraying process follows the following standards: 1. "Code for Construction of Anti-corrosion of Water Transport Engineering Structures" JTS / T 209-2020; 2. "Technical Specification for External Corrosion Protection of Beach and Offshore Petroleum Engineering" SY / T 4091-2016; 3. "Technical Standard for Anti-corrosion Engineering of Industrial Equipment and Pipelines" GB / T 50726-2023.
[0055] The steel components sprayed with the magnetic plastic marine composite anticorrosive material in Examples 1 to 5 and the scratch tester were placed in a constant temperature box (temperature of -20°C ± 2°C). After 1 hour, the magnetic plastic marine composite anticorrosive material on the steel component was quickly scratched with the scratch tester in the constant temperature box to make 4 parallel lines with a depth of 25 mm and a depth to the surface of the steel structure, and then another 4 parallel lines were drawn in the vertical direction to form a square grid. The magnetic plastic marine composite anticorrosive material surrounded by the scratches was checked for shedding. The results are shown in the following table:
[0056] Sources Whether it falls off Eligibility Example 1 No shedding qualified Example 2 No shedding qualified Example 3 No shedding qualified Example 4 No shedding qualified Example 5 No shedding qualified
[0057] The rust levels of Examples 1 to 5 were tested in accordance with GB / T32119-2023 Corrosion Control Technology for Multi-layer Mineral Fat Coating of Marine Steel Structures. The results are shown in the following table:
[0058] Sources Rust degree (%) grade Example 1 0 A Example 2 0 A Example 3 0 A Example 4 0 A Example 5 0 A
[0059] The above-described embodiments are compared with the technical solutions and beneficial effects of the present invention, and it should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a magnetic plastic marine composite anti-corrosion material, It is characterized in that The preparation method comprises the following steps: S1: adding the ferromagnetic material into the molten polyethylene wax and mixing and stirring at a speed of 200 r / min to 400 r / min for 20 min to 30 min, and cooling and granulating after the stirring to obtain the matrix layer material; S2: low-density polyethylene LDPE with a number average molecular weight of 14000-18000, a particle size of 60 μm-100 μm, and a drop melting point of 160°C-220°C is used as the protective layer material; S3: spraying the matrix layer material on the surface of the steel component, and then spraying the protective layer material on the surface of the matrix layer material on the steel component for curing to obtain the magnetic plastic marine composite anti-corrosion material.
2. A method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The diameter of the ferromagnetic material is 10 μm to 20 μm.
3. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The ferromagnetic material is ferrite, neodymium iron boron or iron cobalt nickel.
4. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The number average molecular weight of the polyethylene wax is 8000-12000, and the drop melting point of the polyethylene wax is 120°C-140°C.
5. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The melting temperature of the molten polyethylene wax is 120°C to 140°C.
6. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The added amount of the ferromagnetic material is 0.1% to 0.5% of the mass of the polyethylene wax.
7. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The container for mixing and stirring the ferromagnetic material and the molten polyethylene wax includes an aluminum container or a copper container.
8. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The thickness of the matrix layer material sprayed on the surface of the steel component is 0.2mm-0.4mm.
9. The method for preparing a magnetic plastic marine composite anticorrosive material according to claim 1, It is characterized in that The mass ratio of the polyethylene wax to the low-density polyethylene LDPE is 1:
3.
10. A magnetic plastic marine composite anti-corrosion material prepared by the method for preparing a magnetic plastic marine composite anti-corrosion material according to any one of claims 1 to 9.
Citation Information
Patent Citations
High-temperature-resistant magnetic wax anticorrosive material and preparation method thereof
CN110746674A
Petrolatum anti-corrosion adhesive tape and anti-corrosion structure comprising same
CN114316819A