Formula of coating with high self-cleaning property

Through high-shear emulsification, cold plasma treatment and microwave-assisted heating technology, combined with optimized resin and pigment formulas, the problems of self-cleaning coatings in terms of pigment uniform dispersion, adhesion and weather resistance are solved, and efficient coating film adhesion is achieved. Strength and anti-fouling properties extend the service life of the coating film.

CN118755319AInactive Publication Date: 2024-10-11东红科技(东莞)有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411115622.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing self-cleaning coatings have shortcomings in uniform pigment dispersion, film adhesion, weather resistance and environmental protection, making it difficult to effectively solve the problem of adhesive pollution.

Method used

A combination of high-shear emulsification, cold plasma treatment, ultrasonic dispersion and microwave-assisted heating technology is used to optimize the formula of resin and pigments. Through multi-step dispersion technology of additives, the uniformity, adhesion and anti-fouling performance of the coating are improved.

Benefits of technology

Significantly improves the uniformity and stability of the coating, enhances the adhesion and durability of the coating film, improves hydrophobicity and antifouling properties, extends the service life of the coating film, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755319A_ABST
    Figure CN118755319A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and discloses a high-self-cleaning coating formula which comprises, by weight, 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent and 3.2-4.8 parts of auxiliaries, and further discloses a preparation method of the high-self-cleaning coating. Comprising 50-73 parts of resin, 10-20 parts of a pigment, 32-36 parts of a solvent and 3.2-4.8 parts of an auxiliary agent. S2, preliminarily mixing the resin and the solvent: mixing 15 to 20 parts of polyurethane resin, 8 to 15 parts of thermosetting acrylic resin, 5 to 8 parts of fully etherified amino resin, 25 to 30 parts of fluorocarbon resin and 4.5 to 5.5 parts of cyclohexanone; through combination of high-shear emulsification, cold plasma treatment, ultrasonic dispersion and microwave-assisted heating technologies, the dispersion effect of the coating is remarkably improved, and through an optimized resin formula and an efficient preparation process, the coating has excellent weather resistance and corrosion resistance, the service life of a coating film is prolonged, and the service life of the coating film is prolonged. Meanwhile, the water boiling resistance is excellent, the interlayer adhesive force is excellent, and recoating can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a high self-cleaning coating formula. Background Art

[0002] Self-cleaning paint can be used on the surface of substrates (such as glass, ceramics, wood, stone, etc.). It relies on the hydrophobic and hydrophilic physical properties of the paint itself to play an anti-fouling and easy-to-clean (commercially known as self-cleaning) role.

[0003] The contamination of the coating can be divided into two categories: inhalation pollution and adhesion pollution. Inhalation pollution can be prevented from penetrating pollutants by increasing the density of the coating. For example, the Dabao oil-based anti-fouling exterior wall paint of Dabao Paint Co., Ltd. in Taiwan, China; the advanced acrylic exterior wall protective paint of Sankeshu Paint Co., Ltd.; and the advanced solvent-based exterior wall paint of Carpoly Chemical Group Co., Ltd. However, there is no effective solution for adhesion pollution. People have been looking forward to developing self-cleaning coatings that are not easy to adhere to pollution or that can remove attached pollutants with the help of external natural conditions such as rain and wind.

[0004] At present, in terms of improving the self-cleaning property of coatings, there are mainly theories and technologies such as micronization technology, lotus leaf effect, balloon ceramic theory, self-stratification technology and photocatalytic effect. Adhesive pollution can be improved by improving the surface characteristics of the coating. By increasing or decreasing the water contact angle of the coating surface, the coating surface is made hydrophobic (lotus leaf effect) or hydrophilic, which is the two major directions to achieve the anti-fouling and self-cleaning functions of the coating. However, the existing technology still has deficiencies in terms of uniform dispersion of pigments, adhesion of the coating, weather resistance and environmental protection, and further improvement and optimization are urgently needed. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a highly self-cleaning coating formula, which solves the problems of the self-cleaning coating in terms of uniform pigment dispersion, coating film adhesion, weather resistance and environmental protection.

[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high self-cleaning coating formula, calculated by weight, includes 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent and 3.2-4.8 parts of additives.

[0007] Preferably, the resin comprises, by weight, 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin, and 25-30 parts of fluorocarbon resin.

[0008] Preferably, the pigment is an electron transfer type organic compound.

[0009] Preferably, the solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone.

[0010] Preferably, the auxiliary agent comprises, by weight, 0.8-1.2 parts of leveling agent, 1.7-2.3 parts of defoaming agent and 0.7-1.3 parts of dispersant.

[0011] Preferably, the defoaming agent is a silicon-based defoaming agent, and the dispersant is a high molecular copolymer alkyl ammonium salt dispersant.

[0012] A method for preparing a highly self-cleaning coating comprises the following steps:

[0013] S1. Ingredient preparation: prepare various raw materials by weight, including 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent, and 3.2-4.8 parts of additives;

[0014] S2, preliminary mixing of resin and solvent: 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin and 25-30 parts of fluorocarbon resin are mixed with 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone in a high shear emulsifier at 2000-3000 r / min for 15-20 min;

[0015] S3. Surface modification of pigment: 10-20 parts of electron transfer type organic compound pigment are surface modified by cold plasma treatment technology, and the treatment time is 5-10 minutes;

[0016] S4, pigment dispersion: add the surface modified pigment to the mixed resin and solvent, and use ultrasonic dispersion technology to treat for 10-20 minutes;

[0017] S5. Adding additives: add 0.8-1.2 parts of leveling agent, 1.7-2.3 parts of silicone defoamer and 0.7-1.3 parts of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly;

[0018] S6, microwave-assisted dispersion: After ultrasonic dispersion, microwave-assisted heating technology is used to further disperse evenly, the processing time is 10-15 minutes, and the microwave power is controlled at 500-700W;

[0019] S7, spray drying: the uniformly mixed coating is dried by spray drying equipment, the drying temperature is controlled at 60-80°C, and the drying rate is 5-10ml / min;

[0020] S8, particle refinement: the spray-dried coating particles are refined by jet milling technology, and the processing time is 10-15 minutes;

[0021] S9, finished paint: collect the refined paint particles and filter them through a 300-mesh filter to obtain the finished paint.

[0022] Preferably, the step S6 specifically includes the following steps:

[0023] S6.1. Place the mixed coating in a microwave-assisted dispersion device, and control the microwave power at 500-700W;

[0024] S6.2. The processing time is 10-15 minutes, with intermittent heating, each heating time is 2-3 minutes, with an interval of 1-2 minutes.

[0025] The invention provides a highly self-cleaning coating formula, which has the following beneficial effects:

[0026] 1. The present invention significantly improves the dispersion effect of the coating through a combination of high shear emulsification, cold plasma treatment, ultrasonic dispersion and microwave-assisted heating technology. The pigment and resin can be fully mixed at the molecular level, avoiding the agglomeration of the pigment, improving the uniformity and stability of the coating, and making it have excellent adhesion to various metal substrates.

[0027] 2. The present invention uses cold plasma treatment technology to modify the surface of the pigment, thereby increasing the surface energy of the pigment and enhancing its bonding with the resin, which not only improves the color vividness and durability of the coating, but also improves the chemical stability of the coating, making the coating bright in color and having good colorability.

[0028] 3. The present invention ensures uniform distribution of additives in the coating through multi-step dispersion technology, improves the fluidity of the coating and the flatness of the coating, reduces the generation of bubbles and other defects, and the fluorocarbon resin and surface-modified pigments in the coating formula make the coating surface have excellent hydrophobicity and anti-fouling properties. Dirt is not easy to adhere to the surface of the coating, which is more convenient to clean and reduces maintenance costs.

[0029] 4. The present invention has an optimized resin formula and an efficient preparation process, so that the coating has excellent weather resistance and corrosion resistance, can be used outdoors and in harsh environments for a long time, extends the service life of the coating film, has excellent water boiling resistance, and has excellent interlayer adhesion and can be recoated. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Please refer to the attached Figure 1 The embodiment of the present invention provides a high self-cleaning coating formula, which includes 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent and 3.2-4.8 parts of additives by weight.

[0033] The resin comprises, by weight, 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin and 25-30 parts of fluorocarbon resin.

[0034] Pigments are electron transfer type organic compounds.

[0035] The solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone.

[0036] The additives include, by weight, 0.8-1.2 parts of leveling agent, 1.7-2.3 parts of defoaming agent and 0.7-1.3 parts of dispersant.

[0037] The dispersant is a high molecular copolymer alkyl ammonium salt dispersant.

[0038] A method for preparing a highly self-cleaning coating comprises the following steps:

[0039] S1. Ingredient preparation: prepare various raw materials by weight, including 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent, and 3.2-4.8 parts of additives;

[0040] S2, preliminary mixing of resin and solvent: 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin and 25-30 parts of fluorocarbon resin are mixed with 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone in a high shear emulsifier at 2000-3000 r / min for 15-20 min;

[0041] S3. Surface modification of pigment: 10-20 parts of electron transfer type organic compound pigment are surface modified by cold plasma treatment technology, and the treatment time is 5-10 minutes;

[0042] S4, pigment dispersion: add the surface modified pigment to the mixed resin and solvent, and use ultrasonic dispersion technology to treat for 10-20 minutes;

[0043] S5. Adding additives: add 0.8-1.2 parts of leveling agent, 1.7-2.3 parts of silicone defoamer and 0.7-1.3 parts of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly;

[0044] S6, microwave-assisted dispersion: After ultrasonic dispersion, microwave-assisted heating technology is used to further disperse evenly, the processing time is 10-15 minutes, and the microwave power is controlled at 500-700W;

[0045] S7, spray drying: the uniformly mixed coating is dried by spray drying equipment, the drying temperature is controlled at 60-80°C, and the drying rate is 5-10ml / min;

[0046] S8, particle refinement: the spray-dried coating particles are refined by jet milling technology, and the processing time is 10-15 minutes;

[0047] S9, finished paint: collect the refined paint particles and filter them through a 300-mesh filter to obtain the finished paint.

[0048] Step S6 specifically includes the following steps:

[0049] S6.1. Place the mixed coating in a microwave-assisted dispersion device, and control the microwave power at 500-700W;

[0050] S6.2. The processing time is 10-15 minutes, with intermittent heating, each heating time is 2-3 minutes, with an interval of 1-2 minutes.

[0051] Embodiment 1:

[0052] formula:

[0053] Resin:

[0054] Polyurethane resin: 15 parts

[0055] Thermosetting acrylic resin: 8 parts

[0056] Fully etherified amino resin: 5 parts

[0057] Fluorocarbon resin: 25 parts

[0058] Pigment: 10 parts

[0059] Solvent:

[0060] Cyclohexanone: 4.5 parts

[0061] Xylene: 7.5 parts

[0062] Butyl ester: 11.5 parts

[0063] Methyl isobutyl ketone: 8.5 parts

[0064] Additives:

[0065] Leveling agent: 0.8 parts

[0066] Defoamer: 1.7 parts

[0067] Dispersant: 0.7 parts

[0068] Preparation method:

[0069] S1. Ingredients preparation:

[0070] Prepare 53 parts of resin, 10 parts of pigment, 32 parts of solvent, and 3.2 parts of auxiliary agent by weight.

[0071] S2. Preliminary mixing of resin and solvent:

[0072] 15 parts of polyurethane resin, 8 parts of thermosetting acrylic resin, 5 parts of fully etherified amino resin and 25 parts of fluorocarbon resin were mixed with 4.5 parts of cyclohexanone, 7.5 parts of xylene, 11.5 parts of butyl ester and 8.5 parts of methyl isobutyl ketone in a high shear emulsifier at 2500 r / min for 20 minutes.

[0073] S3. Surface modification of pigments:

[0074] 10 parts of the electron transfer type organic compound pigment were surface modified by cold plasma treatment technology, and the treatment time was 7 minutes.

[0075] S4. Pigment dispersion:

[0076] The surface-modified pigment was added to the mixed resin and solvent and treated using ultrasonic dispersion technology for 15 minutes.

[0077] S5. Addition of additives:

[0078] Add 0.8 parts of leveling agent, 1.7 parts of silicone defoamer and 0.7 parts of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly.

[0079] S6. Microwave assisted dispersion:

[0080] The mixed coating was placed in a microwave-assisted dispersion device, the microwave power was controlled at 600 W, the processing time was 12 minutes, and intermittent heating was performed, each heating was 2 minutes, and the interval was 1 minute.

[0081] S7, spray drying:

[0082] The uniformly mixed coating was dried by spray drying equipment, with the drying temperature controlled at 70°C and the drying rate at 5 ml / min.

[0083] S8, particle refinement:

[0084] The spray-dried coating particles were finely processed by jet milling technology for 12 minutes.

[0085] S9, Finished coating:

[0086] The refined paint particles are collected and filtered through a 300-mesh filter to obtain a finished paint.

[0087] Summarize:

[0088] This embodiment ensures uniform dispersion of resin and pigment through high shear emulsification and cold plasma treatment technology, enhances the binding force between pigment and resin, and makes the coating film bright in color, with excellent hydrophobicity and antifouling properties.

[0089] Embodiment 2:

[0090] formula:

[0091] Resin:

[0092] Polyurethane resin: 20 parts

[0093] Thermosetting acrylic resin: 15 parts

[0094] Fully etherified amino resin: 8 parts

[0095] Fluorocarbon resin: 30 parts

[0096] Pigment: 20 parts

[0097] Solvent:

[0098] Cyclohexanone: 5.5 parts

[0099] Xylene: 8.5 parts

[0100] Butyl ester: 12.5 parts

[0101] Methyl isobutyl ketone: 9.5 parts

[0102] Additives:

[0103] Leveling agent: 1.2 parts

[0104] Defoamer: 2.3 parts

[0105] Dispersant: 1.3 parts

[0106] Preparation method:

[0107] S1. Ingredients preparation:

[0108] Prepare 73 parts of resin, 20 parts of pigment, 36 parts of solvent and 4.8 parts of auxiliary agent by weight.

[0109] S2. Preliminary mixing of resin and solvent:

[0110] 20 parts of polyurethane resin, 15 parts of thermosetting acrylic resin, 8 parts of fully etherified amino resin and 30 parts of fluorocarbon resin were mixed with 5.5 parts of cyclohexanone, 8.5 parts of xylene, 12.5 parts of butyl ester and 9.5 parts of methyl isobutyl ketone in a high shear emulsifier at 2500 r / min for 20 minutes.

[0111] S3. Surface modification of pigments:

[0112] 20 parts of the electron transfer type organic compound pigment were surface modified by cold plasma treatment technology, and the treatment time was 7 minutes.

[0113] S4. Pigment dispersion:

[0114] The surface-modified pigment was added to the mixed resin and solvent and treated using ultrasonic dispersion technology for 15 minutes.

[0115] S5. Addition of additives:

[0116] Add 1.2 parts of leveling agent, 2.3 parts of silicone defoamer and 1.3 parts of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly.

[0117] S6. Microwave assisted dispersion:

[0118] The mixed coating was placed in a microwave-assisted dispersion device, the microwave power was controlled at 600 W, the processing time was 12 minutes, and intermittent heating was performed, each heating was 2 minutes, and the interval was 1 minute.

[0119] S7, spray drying:

[0120] The uniformly mixed coating was dried by spray drying equipment, with the drying temperature controlled at 70°C and the drying rate at 5 ml / min.

[0121] S8, particle refinement:

[0122] The spray-dried coating particles were finely processed by jet milling technology for 12 minutes.

[0123] S9, Finished coating:

[0124] The refined paint particles are collected and filtered through a 300-mesh filter to obtain a finished paint.

[0125] Summarize:

[0126] In this embodiment, the dosage of resin and pigment is relatively high, and the thickness and adhesion of the coating film are further improved, which is suitable for application scenarios with higher requirements for mechanical properties.

[0127] Embodiment 3:

[0128] formula:

[0129] Resin:

[0130] Polyurethane resin: 14 parts

[0131] Thermosetting acrylic resin: 10 parts

[0132] Fully etherified amino resin: 5 parts

[0133] Fluorocarbon resin: 20 parts

[0134] Pigment: 15 parts

[0135] Solvent:

[0136] Cyclohexanone: 5 parts

[0137] Xylene: 8 parts

[0138] Butyl ester: 12 parts

[0139] Methyl isobutyl ketone: 9 parts

[0140] Additives:

[0141] Leveling agent: 1 part

[0142] Defoaming agent: 2 parts

[0143] Dispersant: 1 part

[0144] Preparation method:

[0145] S1. Ingredients preparation:

[0146] Prepare 49 parts of resin, 15 parts of pigment, 34 parts of solvent and 4 parts of auxiliary agent by weight.

[0147] S2. Preliminary mixing of resin and solvent:

[0148] 14 parts of polyurethane resin, 10 parts of thermosetting acrylic resin, 5 parts of fully etherified amino resin and 20 parts of fluorocarbon resin were mixed with 5 parts of cyclohexanone, 8 parts of xylene, 12 parts of butyl ester and 9 parts of methyl isobutyl ketone in a high shear emulsifier at 2500 r / min for 20 minutes.

[0149] S3. Surface modification of pigments:

[0150] 15 parts of the electron transfer type organic compound pigment were surface modified by cold plasma treatment technology, and the treatment time was 7 minutes.

[0151] S4. Pigment dispersion:

[0152] The surface-modified pigment was added to the mixed resin and solvent and treated using ultrasonic dispersion technology for 15 minutes.

[0153] S5. Addition of additives:

[0154] Add 1 part of leveling agent, 2 parts of silicone defoamer and 1 part of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly.

[0155] S6. Microwave assisted dispersion:

[0156] The mixed coating was placed in a microwave-assisted dispersion device, the microwave power was controlled at 600 W, the processing time was 12 minutes, and intermittent heating was performed, each heating was 2 minutes, and the interval was 1 minute.

[0157] S7, spray drying:

[0158] The uniformly mixed coating was dried by spray drying equipment, with the drying temperature controlled at 70°C and the drying rate at 5 ml / min.

[0159] S8, particle refinement:

[0160] The spray-dried coating particles were finely processed by jet milling technology for 12 minutes.

[0161] S9, Finished coating:

[0162] The refined paint particles are collected and filtered through a 300-mesh filter to obtain a finished paint.

[0163] Summarize:

[0164] The resin and pigment dosage of this embodiment is moderate, and the adhesion and self-cleaning properties of the coating are balanced, which is suitable for general industrial and civilian scenarios.

[0165] Summary:

[0166] The three embodiments differ in formulation and dosage, and are optimized for different application scenarios and performance requirements:

[0167] Example 1: The formula is balanced and suitable for a wide range of industrial applications, with excellent self-cleaning properties and hydrophobicity.

[0168] Example 2: The amount of resin and pigment used is higher, the coating thickness and adhesion are stronger, and it is suitable for scenes with higher requirements for mechanical properties.

[0169] Example 3: The dosage is moderate, taking into account both self-cleaning performance and adhesion, and is suitable for general industrial and civilian use.

[0170] Test experiment and its contents:

[0171] Purpose:

[0172] The performance of high self-cleaning coatings of three different formulations was comprehensively evaluated in terms of adhesion, hydrophobicity, anti-fouling performance, weather resistance, corrosion resistance, mechanical properties (such as hardness and wear resistance), and self-cleaning effect, to verify the effectiveness and superiority of each formulation and find the coating formulation most suitable for different application scenarios.

[0173] Experimental content and experimental contents:

[0174] 1. Coating adhesion test

[0175] Purpose: To evaluate the adhesion of coatings on different substrates. Procedure:

[0176] The coatings from each formulation were applied to metal, glass, ceramic and wood panels.

[0177] Use the cross-hatch method (ASTM D3359) to draw a grid on the coating film.

[0178] Use special tape to stick on the grid, tear it off quickly, and observe the integrity of the grid.

[0179] The adhesion of each coating on the different substrates was recorded.

[0180] 2. Hydrophobicity test

[0181] Purpose: To evaluate the hydrophobicity of the coating. Procedure:

[0182] The coatings of each formulation were coated on glass plates and tested after curing.

[0183] Use a burette to drop a drop of water on the coating surface and measure the contact angle of the water drop.

[0184] Measure the contact angles at different locations and take the average value.

[0185] 3. Antifouling performance test

[0186] Purpose: To evaluate the antifouling ability of the coating. Steps:

[0187] The coatings of each formulation were coated on glass plates and tested after curing.

[0188] Apply the same amount of stain (such as oil-based marker, coffee, red wine, etc.) on the surface of the coating.

[0189] After 24 hours, wipe with a damp cloth and observe the stain removal.

[0190] The ease of cleaning and residual staining of each paint were recorded.

[0191] 4. Weather resistance test

[0192] Purpose: To evaluate the weather resistance of coatings in harsh environments. Steps:

[0193] The coatings of each formulation were applied on metal plates and tested after curing.

[0194] The samples were placed in a UV accelerated aging test chamber for UV irradiation and humidity and heat cycling (according to ASTM G154 standard).

[0195] Samples were taken out every 100 hours to observe the color changes and physical property changes of the coating.

[0196] Record the changes in each coating at different aging time points.

[0197] 5. Corrosion resistance test

[0198] Purpose: To evaluate the corrosion resistance of the coating in a corrosive environment. Steps:

[0199] The coatings of each formulation were applied on metal plates and tested after curing.

[0200] Place the sample in a salt spray test chamber (according to ASTM B117 standard).

[0201] Samples were taken out every 100 hours to observe the corrosion of the coating.

[0202] Record the changes of each coating at different corrosion time points.

[0203] 6. Mechanical properties test

[0204] Purpose: To evaluate the mechanical properties of the coating, such as hardness and wear resistance. Procedure:

[0205] The coatings of each formulation were applied on metal plates and tested after curing.

[0206] The hardness of the coating film was evaluated using a pencil hardness test (ASTM D3363).

[0207] The abrasion resistance of the coatings was evaluated using a Taber abrasion tester with a CS-10 abrasive wheel and a 1000 g load.

[0208] The hardness and abrasion of each coating were recorded.

[0209] 7. Self-cleaning effect test

[0210] Purpose: To evaluate the self-cleaning effect of the coating. Steps:

[0211] The coatings of each formulation were coated on glass plates and tested after curing.

[0212] Apply the same amount of mud on the coating surface and rinse with water after drying.

[0213] Observe the amount of mud remaining on the coating surface and evaluate the self-cleaning effect.

[0214] The self-cleaning performance of each coating was recorded.

[0215] Table 1:

[0216]

[0217]

[0218]

[0219] Test experiment summary:

[0220] Example 1: It has good adhesion and hydrophobicity, excellent antifouling performance, good weather resistance and corrosion resistance, moderate mechanical properties, significant self-cleaning effect, and is suitable for general industrial applications.

[0221] Example 2: It performs well in all test items, especially in weather resistance, corrosion resistance and mechanical properties, and is suitable for demanding outdoor and industrial applications.

[0222] Example 3: The adhesion and hydrophobicity are good, but the weather resistance and corrosion resistance are slightly inferior to the previous two, the mechanical properties are slightly lower, the self-cleaning effect is good, and it is suitable for general industrial and civilian scenarios.

[0223] Comparative experiment and its experimental content:

[0224] Purpose:

[0225] Evaluate the advantages of the highly self-cleaning coating prepared by the present invention over traditional coatings in terms of adhesion, hydrophobicity, antifouling performance, weather resistance, corrosion resistance, mechanical properties (such as hardness and wear resistance) and self-cleaning effect.

[0226] Experimental content and steps

[0227] Paint samples:

[0228] Coatings of the present invention: Example 1, Example 2, Example 3

[0229] Traditional coating A: Commercially available ordinary acrylic exterior wall coating

[0230] Traditional coating B: Commercially available fluorocarbon coating

[0231] Traditional coating C: Commercially available nano self-cleaning coating

[0232] 1. Coating adhesion test

[0233] Purpose: To evaluate the adhesion of coatings on different substrates.

[0234] step:

[0235] The coatings from each formulation were applied to metal, glass, ceramic and wood panels.

[0236] Use the cross-hatch method (ASTM D3359) to draw a grid on the coating film.

[0237] Use special tape to stick on the grid, tear it off quickly, and observe the integrity of the grid.

[0238] The adhesion of each coating on the different substrates was recorded.

[0239] 2. Hydrophobicity test

[0240] Purpose: To evaluate the hydrophobicity of coatings.

[0241] step:

[0242] The coatings of each formulation were coated on glass plates and tested after curing.

[0243] Use a burette to drop a drop of water on the coating surface and measure the contact angle of the water drop.

[0244] Measure the contact angles at different locations and take the average value.

[0245] 3. Antifouling performance test

[0246] Purpose: To evaluate the antifouling ability of coatings.

[0247] step:

[0248] The coatings of each formulation were coated on glass plates and tested after curing.

[0249] Apply the same amount of stain (such as oil-based marker, coffee, red wine, etc.) on the surface of the coating.

[0250] After 24 hours, wipe with a damp cloth and observe the stain removal.

[0251] The ease of cleaning and residual staining of each paint were recorded.

[0252] 4. Weather resistance test

[0253] Purpose: To evaluate the weather resistance of coatings in harsh environments.

[0254] step:

[0255] The coatings of each formulation were applied on metal plates and tested after curing.

[0256] The samples were placed in a UV accelerated aging test chamber for UV irradiation and humidity and heat cycling (according to ASTM G154 standard).

[0257] Samples were taken out every 100 hours to observe the color changes and physical property changes of the coating.

[0258] Record the changes in each coating at different aging time points.

[0259] 5. Corrosion resistance test

[0260] Purpose: To evaluate the corrosion resistance of coatings in corrosive environments.

[0261] step:

[0262] The coatings of each formulation were applied on metal plates and tested after curing.

[0263] Place the sample in a salt spray test chamber (according to ASTM B117 standard).

[0264] Samples were taken out every 100 hours to observe the corrosion of the coating.

[0265] Record the changes of each coating at different corrosion time points.

[0266] 6. Mechanical properties test

[0267] Purpose: To evaluate the mechanical properties of coatings, such as hardness and wear resistance.

[0268] step:

[0269] The coatings of each formulation were applied on metal plates and tested after curing.

[0270] The hardness of the coating film was evaluated using a pencil hardness test (ASTM D3363).

[0271] The abrasion resistance of the coatings was evaluated using a Taber abrasion tester with a CS-10 abrasive wheel and a 1000 g load.

[0272] The hardness and abrasion of each coating were recorded.

[0273] 7. Self-cleaning effect test

[0274] Purpose: To evaluate the self-cleaning effect of coatings.

[0275] step:

[0276] The coatings of each formulation were coated on glass plates and tested after curing.

[0277] Apply the same amount of mud on the coating surface and rinse with water after drying.

[0278] Observe the amount of mud remaining on the coating surface and evaluate the self-cleaning effect.

[0279] The self-cleaning performance of each coating was recorded.

[0280] Table 2:

[0281]

[0282]

[0283]

[0284] Experimental summary:

[0285] Adhesion: The adhesion of the coating of the present invention on various substrates is significantly better than that of traditional coatings, especially on glass and ceramic substrates. It is suitable for a variety of application scenarios and is widely used in surface decoration and protection of industrial products such as stainless steel, aluminum alloy, cast iron, and bakelite.

[0286] Hydrophobicity: The hydrophobicity of the coating of the present invention is significantly better than that of traditional coatings, with a larger contact angle, showing excellent waterproof and self-cleaning effects.

[0287] Antifouling performance: The coating of the present invention performs excellently in the antifouling performance test, the stains are easy to clean, and the residue is small, which is significantly better than traditional coatings.

[0288] Weather resistance: The coating of the present invention performs well in the ultraviolet accelerated aging test, has good weather resistance, and has little change in the physical properties of the coating film under long-term exposure, making it suitable for outdoor applications.

[0289] Corrosion resistance: The coating of the present invention shows excellent corrosion resistance in the salt spray test, and the corrosion degree of the coating film is low, and is suitable for use in corrosive environments.

[0290] Mechanical properties: The coating of the present invention performs well in hardness and wear resistance tests, and its mechanical properties are significantly improved, making it suitable for high wear environments.

[0291] Self-cleaning effect: The self-cleaning performance of the coating of the present invention is significantly better than that of traditional coatings, with less mud residue, easy cleaning and low maintenance cost.

[0292] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A highly self-cleaning coating formulation, characterized in that: By weight, it comprises 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent and 3.2-4.8 parts of auxiliary agent.

2. A highly self-cleaning coating formulation according to claim 1, characterized in that: The resin comprises, by weight, 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin, and 25-30 parts of fluorocarbon resin.

3. A highly self-cleaning coating formulation according to claim 1, characterized in that: The pigment is an electron transfer type organic compound.

4. A highly self-cleaning coating formulation according to claim 1, characterized in that: The solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone.

5. A highly self-cleaning coating formulation according to claim 1, characterized in that: The auxiliary agent comprises, by weight, 0.8-1.2 parts of a leveling agent, 1.7-2.3 parts of a defoaming agent and 0.7-1.3 parts of a dispersant.

6. A highly self-cleaning coating formulation according to claim 5, characterized in that: The defoamer is a silicon-based defoamer, and the dispersant is a high molecular copolymer alkyl ammonium salt-based dispersant.

7. A method for preparing a highly self-cleaning coating, characterized in that: The method is prepared by using a high self-cleaning coating formulation as described in any one of claims 1 to 6, comprising the following steps: S1. Ingredient preparation: prepare various raw materials by weight, including 50-73 parts of resin, 10-20 parts of pigment, 32-36 parts of solvent, and 3.2-4.8 parts of additives; S2, preliminary mixing of resin and solvent: 15-20 parts of polyurethane resin, 8-15 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin and 25-30 parts of fluorocarbon resin are mixed with 4.5-5.5 parts of cyclohexanone, 7.5-8.5 parts of xylene, 11.5-12.5 parts of butyl ester and 8.5-9.5 parts of methyl isobutyl ketone in a high shear emulsifier at 2000-3000 r / min for 15-20 min; S3. Surface modification of pigment: 10-20 parts of electron transfer type organic compound pigment are surface modified by cold plasma treatment technology, and the treatment time is 5-10 minutes; S4, pigment dispersion: add the surface modified pigment to the mixed resin and solvent, and use ultrasonic dispersion technology to treat for 10-20 minutes; S5. Adding additives: add 0.8-1.2 parts of leveling agent, 1.7-2.3 parts of silicone defoamer and 0.7-1.3 parts of high molecular copolymer alkyl ammonium dispersant, and continue to stir evenly; S6, microwave-assisted dispersion: After ultrasonic dispersion, microwave-assisted heating technology is used to further disperse evenly, the processing time is 10-15 minutes, and the microwave power is controlled at 500-700W; S7, spray drying: the uniformly mixed coating is dried by spray drying equipment, the drying temperature is controlled at 60-80°C, and the drying rate is 5-10ml / min; S8, particle refinement: the spray-dried coating particles are refined by jet milling technology, and the processing time is 10-15 minutes; S9, finished paint: collect the refined paint particles and filter them through a 300-mesh filter to obtain the finished paint.

8. The method for preparing a highly self-cleaning coating according to claim 7, characterized in that: The step S6 specifically includes the following steps: S6.

1. Place the mixed coating in a microwave-assisted dispersion device, and control the microwave power at 500-700W; S6.

2. The processing time is 10-15 minutes, with intermittent heating, each heating time is 2-3 minutes, with an interval of 1-2 minutes.

Citation Information

Patent Citations

  • Low-temperature plasma modified aluminum oxide enhanced phenolic resin and preparation method thereof

    CN103525003A

  • Anti-sticking coating

    CN107459919A

  • Self cleaning paint

    CN107502080A

  • Superfine powder paint and its prepn process

    CN1706891A

  • Power coating material and method for forming coated film

    JP2003105265A