Waterborne epoxy mica iron oxide paint and production method thereof
By modifying the epoxy resin emulsion to generate silanol groups, combined with chopped fibers and modified polyhydroxyalkanoate, the problem of low coating adhesion in water-based insulation coatings is solved, and the adhesion and adhesion of the coating are improved. Heat and cold resistance.
Patent Information
- Application Number
- CN202410985439.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Water-based insulating coatings require the use of a large amount of inorganic fillers, resulting in low coating adhesion and poor resistance to cold and heat cycles.
By modifying the epoxy resin emulsion to generate silanol groups (Si-OH), forming chemical bonds with the hydroxyl groups (OH) on the surface of the substrate, and adding chopped fibers and modified polyhydroxyalkanoate to the coating, Modified with hollow glass fibers to enhance the adhesion and flexibility of the coating.
It improves the adhesion and resistance to cold and heat cycles of the coating, avoids bulging and cracking of the coating, and enhances the strength and environmental adaptability of the coating.
Smart Images

Figure CN118755348A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterborne epoxy paint, in particular to a waterborne epoxy mica iron oxide paint and a production method thereof. Background Art
[0002] Water-based epoxy mica iron oxide paint is an environmentally friendly paint that uses water as a diluent and does not contain toxic and harmful ingredients such as organic solvents. It is safe and environmentally friendly. This paint is widely used in anti-corrosion decoration of ships, bridges, steel structures, towers, container bodies, etc. Since a large amount of inorganic fillers are required in water-based insulating paints, the coating is prone to low adhesion and poor resistance to cold and hot cycles. How to ensure the insulation of the coating while maintaining the stability of the coating is a problem that needs to be addressed. Summary of the invention
[0003] The purpose of the present invention is to provide a water-based epoxy mica iron oxide paint and a production method thereof, by modifying the epoxy resin emulsion to generate silanol groups (Si-OH), which can form chemical bonds with the hydroxyl groups (OH) on the surface of the substrate, thereby improving the adhesion of the coating and solving the problems raised in the above-mentioned background technology.
[0004] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a water-based epoxy mica iron oxide paint, comprising component A and component B, wherein the solid content of component A and component B is more than 50%, component A comprises the following raw materials in parts by weight: 50-60 parts of modified water-based epoxy resin emulsion, 20-40 parts of mica iron oxide pigment, 4-6 parts of reinforcing material, 0.1-1 parts of auxiliary agent, and 5-40 parts of deionized water; component B comprises the following raw materials in parts by weight: 20-30 parts of water-based phenolic amine curing agent, 0.1-3 parts of triethanolamine and 1-20 parts of deionized water, wherein the reinforcing material comprises chopped fibers and modified polyhydroxyalkanoate.
[0005] Preferably, the preparation method of the modified epoxy resin emulsion is as follows: pour propylene glycol methyl ether into epoxy resin particles, heat to 60-70°C, stir with a magnetic stirrer until the epoxy resin is completely dissolved, pre-dissolve a nonionic surfactant in deionized water to prepare an emulsifier aqueous solution, slowly pour the propylene glycol methyl ether solution containing the resin into the emulsifier aqueous solution, and use a high-speed disperser for variable speed stirring to form an emulsion, add the pretreated silane, and after dispersion and emulsification are completed, cool the emulsion to room temperature and continue stirring until the emulsion is stable.
[0006] Preferably, the ratio of the epoxy resin particles, propylene glycol methyl ether and the emulsifier aqueous solution is 6:3:1.
[0007] Preferably, the silane pretreatment method is as follows: 1-5% of the weight of the epoxy resin particles is mixed with an ethanol aqueous solution, the concentration of the silane is 0.5%, and the pH value is adjusted to 4-6 at room temperature.
[0008] Preferably, the ratio of the chopped fibers to the modified polyhydroxyalkanoate is 2-3:1, and the chopped fibers are modified hollow glass fibers.
[0009] Preferably, the preparation method of the modified hollow glass fiber is as follows:
[0010] In the drawing process of manufacturing glass fiber, gas is introduced to form a hollow structure to make hollow glass fiber. The hollow glass fiber is treated with hydrofluoric acid to corrode part of the surface to form a microporous structure. At the same time, the surface of the glass fiber is activated. The activated glass fiber is immersed in a polyethylene glycol solution, and a catalyst azobisisobutyronitrile is added to initiate a free radical polymerization reaction so that the polymer forms a graft layer directly on the fiber surface. After the reaction is completed, the glass fiber is washed with deionized water to remove unreacted monomers and by-products, and then dried in a vacuum oven to constant weight.
[0011] Preferably, the preparation method of the modified polyhydroxyalkanoate is as follows:
[0012] The polyhydroxyalkanoate particles are immersed in a 0.1M NaIO4 solution and treated at room temperature for 1-2 hours. After the oxidation treatment, the polyhydroxyalkanoate particles are washed with deionized water several times to remove residual NaIO4, and then dried in a vacuum oven to complete the activation of the polyhydroxyalkanoate particles. The activated polyhydroxyalkanoate particles are dispersed in a DCM organic solvent, PEG-NH2 and a catalyst DCC, as well as a small amount of NHS are added to help form a stable amide bond. Under nitrogen protection, the reaction mixture is placed under heating conditions of 40-50°C for reaction for 5-24 hours. After the reaction is completed, the grafted polyhydroxyalkanoate is separated by centrifugation and then washed with ethanol and water to remove unreacted PEG, DCC byproducts and other impurities. Finally, the product is dried under vacuum until the solvent is completely removed to obtain a modified polyhydroxyalkanoate.
[0013] Preferably, the average particle size of the mica iron oxide pigment is less than 5 μm and the purity is greater than 98%.
[0014] Preferably, the auxiliary agent includes at least one of a defoaming agent, a preservative, a pH regulator, a thickener, and a wetting agent.
[0015] Another technical problem to be solved by the present invention is to provide a production method of water-based epoxy mica iron oxide paint, comprising the following steps:
[0016] Step 1: Mix the modified waterborne epoxy resin emulsion and deionized water, dilute the modified waterborne epoxy resin emulsion, and mix the reinforcing material with deionized water for pre-dispersion, and mix the pre-dispersed reinforcing material with the diluted modified waterborne epoxy resin emulsion, use high-speed dispersing equipment to ensure uniform distribution, add mica iron oxide pigment and additives to continue mixing, add deionized water, and adjust the consistency of component A;
[0017] Step 2: Mix the water-based phenolic amine curing agent, triethanolamine and an appropriate amount of deionized water, stir evenly and support component B for later use;
[0018] Step 3: Mix component A and component B, stir well and then apply.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] In summary, the present invention proposes a water-based epoxy mica iron oxide paint and a production method thereof, wherein epoxy resin emulsion is modified to generate silanol groups (Si-OH), so that chemical bonds can be formed with hydroxyl groups (OH) on the surface of a substrate, thereby improving the adhesion of the coating. Short-cut fibers and modified polyhydroxyalkanoate are added to component A, hollow glass fibers are used, and the glass fibers are modified to increase the surface area of the glass fibers, expand the contact area with the epoxy resin emulsion, improve the dispersion effect of the glass fibers, and utilize glass fibers to enhance the strength of the water-based epoxy mica iron oxide paint. At the same time, the modified polyhydroxyalkanoate material introduced increases the flexibility, environmental adaptability and biodegradability of the coating, and the two act synergistically to avoid bulging and cracking of the coating, thereby further improving the adhesion of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Embodiment 1:
[0024] In order to solve the problem that existing water-based insulating coatings need to use a large amount of inorganic fillers, which is prone to low coating adhesion and poor resistance to cold and hot cycles, how to ensure the insulation of the coating while maintaining the stability of the coating is a problem that needs to be solved. Please refer to Figure 1 , this embodiment provides the following technical solutions:
[0025] A water-based epoxy mica iron oxide paint comprises a component A and a component B, wherein the solid content of the component A and the component B is more than 50%.
[0026] Component A includes the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 20 parts of mica iron oxide pigment, 4 parts of reinforcing material, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%, wherein the reinforcing material includes chopped fibers and modified polyhydroxyalkanoate.
[0027] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0028] In the present embodiment, the preparation method of the modified epoxy resin emulsion is as follows: propylene glycol methyl ether is poured into epoxy resin particles, heated to 60-70°C, and stirred using a magnetic stirrer until the epoxy resin is completely dissolved, a nonionic surfactant is pre-dissolved in deionized water to prepare an emulsifier aqueous solution, and the propylene glycol methyl ether solution dissolved with the resin is slowly poured into the emulsifier aqueous solution, and a high-speed disperser is used for variable speed stirring. The initial rapid stirring time is 2-5 minutes, the purpose is to quickly disperse the oil phase, once the colostrum is formed, the stirring speed can be reduced, and the emulsification time can be extended to ensure the uniformity and stability of the emulsion, and an emulsion is formed. The pretreated silane is added. After the dispersion and emulsification are completed, the emulsion is cooled to room temperature and continued to be stirred until the emulsion is stable. The ratio of epoxy resin particles, propylene glycol methyl ether and emulsifier aqueous solution is 6:3:1.
[0029] In this embodiment, the silane pretreatment method is as follows: 2% of the weight of the epoxy resin particles is mixed with an ethanol aqueous solution, the concentration of silane is 0.5%, and the pH value is adjusted to 5 at room temperature. This process can hydrolyze the alkoxy groups on the silane molecules to generate silanol groups (Si-OH), which can form chemical bonds with the hydroxyl groups (OH) on the surface of the substrate, thereby improving the adhesion of the coating.
[0030] In this embodiment, the ratio of the chopped fibers to the modified polyhydroxyalkanoate is 3:1, and the chopped fibers are modified hollow glass fibers.
[0031] In this embodiment, the preparation method of the modified hollow glass fiber is as follows:
[0032] In the drawing process of manufacturing glass fiber, gas is introduced to form a hollow structure to make hollow glass fiber. The hollow glass fiber is treated with hydrofluoric acid to corrode part of the surface to form a microporous structure. At the same time, the surface of the glass fiber is activated. The activated glass fiber is immersed in a polyethylene glycol solution, and a catalyst azobisisobutyronitrile is added to initiate a free radical polymerization reaction so that the polymer forms a graft layer directly on the fiber surface. After the reaction is completed, the glass fiber is washed with deionized water to remove unreacted monomers and by-products, and then dried in a vacuum oven to constant weight.
[0033] In this embodiment, the preparation method of modified polyhydroxyalkanoate is as follows:
[0034] The polyhydroxyalkanoate particles were immersed in a 0.1M NaIO4 solution and treated at room temperature for 1 hour for oxidation treatment to introduce reactive functional groups such as carboxyl groups. After oxidation treatment, the polyhydroxyalkanoate particles were washed with deionized water several times to remove residual NaIO4, and then dried in a vacuum oven to complete the activation of the polyhydroxyalkanoate particles. The activated polyhydroxyalkanoate particles were dispersed in a DCM organic solvent, PEG-NH2 and a catalyst DCC, as well as a small amount of NHS were added to help form a stable amide bond. Under nitrogen protection, the reaction mixture was placed at 45°C for 10 hours for heating to terminate the reaction. Finally, the grafted polyhydroxyalkanoate is separated by centrifugation and then washed with ethanol and water to remove unreacted PEG, DCC byproducts and other impurities. Finally, the product is dried under vacuum until the solvent is completely removed to obtain modified polyhydroxyalkanoate. Hydrophilic groups such as carboxyl groups are grafted on the surface of polyhydroxyalkanoate to improve the biocompatibility, water solubility and compatibility with other materials of polyhydroxyalkanoate, and the dispersibility of polyhydroxyalkanoate in epoxy resin emulsion is improved. As a biodegradable polymer, polyhydroxyalkanoate can improve the flexibility, environmental adaptability and biodegradability of the coating.
[0035] In order to better demonstrate the production process of a water-based epoxy mica iron oxide paint, this embodiment now proposes a production method of a water-based epoxy mica iron oxide paint, comprising the following steps:
[0036] Step 1: Mix the modified waterborne epoxy resin emulsion and deionized water, dilute the modified waterborne epoxy resin emulsion, and mix the reinforcing material with deionized water for pre-dispersion, and mix the pre-dispersed reinforcing material with the diluted modified waterborne epoxy resin emulsion, use high-speed dispersing equipment to ensure uniform distribution, add mica iron oxide pigment and additives to continue mixing, add deionized water, and adjust the consistency of component A;
[0037] Step 2: Mix the water-based phenolic amine curing agent, triethanolamine and an appropriate amount of deionized water, stir evenly and support component B for later use;
[0038] Step 3: Mix component A and component B, stir well and then apply.
[0039] Embodiment 2:
[0040] A water-based epoxy mica iron oxide paint comprises a component A and a component B, wherein the solid content of the component A and the component B is more than 50%.
[0041] Component A includes the following raw materials in parts by weight: 55 parts of modified water-based epoxy resin emulsion, 23 parts of mica iron oxide pigment, 4 parts of reinforcing material, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%, wherein the reinforcing material includes chopped fibers and modified polyhydroxyalkanoate.
[0042] Component B includes the following raw materials in parts by weight: 22 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0043] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0044] Embodiment three:
[0045] A water-based epoxy mica iron oxide paint comprises a component A and a component B, wherein the solid content of the component A and the component B is more than 50%.
[0046] Component A includes the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 20 parts of mica iron oxide pigment, 6 parts of reinforcing material, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%, wherein the reinforcing material includes chopped fibers and modified polyhydroxyalkanoate.
[0047] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0048] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0049] Embodiment 4:
[0050] A water-based epoxy mica iron oxide paint comprises a component A and a component B, wherein the solid content of the component A and the component B is more than 50%.
[0051] Component A includes the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 25 parts of mica iron oxide pigment, 4 parts of reinforcing material, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 25 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%, wherein the reinforcing material includes chopped fibers and modified polyhydroxyalkanoate.
[0052] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0053] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0054] Comparative Example 1:
[0055] The water-based epoxy mica iron oxide paint comprises component A and component B. Component A comprises the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 20 parts of mica iron oxide pigment, 2 parts of chopped fibers, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%.
[0056] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0057] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0058] Comparative Example 2:
[0059] The water-based epoxy mica iron oxide paint comprises component A and component B. Component A comprises the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 20 parts of mica iron oxide pigment, 4 parts of modified polyhydroxyalkanoate, 0.1 parts of defoaming agent, 0.1 parts of preservative, 0.1 parts of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%.
[0060] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0061] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0062] Comparative Example 3:
[0063] The water-based epoxy mica iron oxide paint comprises component A and component B. Component A comprises the following raw materials in parts by weight: 50 parts of modified water-based epoxy resin emulsion, 20 parts of mica iron oxide pigment, 0.1 part of defoaming agent, 0.1 part of preservative, 0.1 part of pH regulator, and 15 parts of deionized water; the average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%.
[0064] Component B includes the following raw materials in parts by weight: 20 parts of water-based phenalkamine curing agent, 0.2 parts of triethanolamine and 6 parts of deionized water.
[0065] The water-based epoxy mica iron oxide paint was prepared in the same manner as in Example 1.
[0066] After mixing Example 1-4 and Comparative Example 1-3 uniformly according to A:B=1:1, the mixture was sprayed on the tinplate sheet at a coating rate of 5.5 m2 / kg. The tinplate sheet was placed in a 15°C constant temperature box to dry for 48 hours to test the conventional performance.
[0067] The following data is obtained:
[0068]
[0069]
[0070] It can be concluded from the above table that the waterborne epoxy mica iron oxide paints prepared in Examples 1 to 4 have little difference in performance. In Example 2, the content of the modified waterborne epoxy resin emulsion is increased, the overall solid content is increased, and the thickness after wet coating and drying is higher than that of other examples. The waterborne epoxy mica iron oxide paint prepared in the comparative example is significantly lower than that of the examples in terms of impact resistance and pull-out adhesion. This is because only a single chopped fiber or modified polyhydroxyalkanoate is used in Comparative Example 1, and no reinforcing material is used in Comparative Example 3, and its impact resistance and pull-out adhesion are relatively weak, indicating that the combination of modified polyhydroxyalkanoate and chopped fibers can produce a synergistic effect. The modified polyhydroxyalkanoate provides flexibility, biodegradability and environmental adaptability, while the fiber enhances the strength and crack resistance of the coating.
[0071] In summary, the present invention proposes a water-based epoxy mica iron oxide paint and a production method thereof, wherein epoxy resin emulsion is modified to generate silanol groups (Si-OH), so that chemical bonds can be formed with hydroxyl groups (OH) on the surface of a substrate, thereby improving the adhesion of the coating. Short-cut fibers and modified polyhydroxyalkanoate are added to component A, hollow glass fibers are used, and the glass fibers are modified to increase the surface area of the glass fibers, expand the contact area with the epoxy resin emulsion, improve the dispersion effect of the glass fibers, and utilize glass fibers to enhance the strength of the water-based epoxy mica iron oxide paint. At the same time, the modified polyhydroxyalkanoate material introduced increases the flexibility, environmental adaptability and biodegradability of the coating, and the two act synergistically to avoid bulging and cracking of the coating, thereby further improving the adhesion of the coating.
[0072] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0073] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
Claims
1. A water-based epoxy mica iron oxide paint, comprising component A and component B, characterized in that: The solid content of the components A and B is more than 50%, the component A comprises the following raw materials in parts by weight: 50-60 parts of modified waterborne epoxy resin emulsion, 20-40 parts of mica iron oxide pigment, 4-6 parts of reinforcing material, 0.1-1 part of auxiliary agent, and 5-40 parts of deionized water; the component B comprises the following raw materials in parts by weight: 20-30 parts of waterborne phenolic amine curing agent, 0.1-3 parts of triethanolamine, and 1-20 parts of deionized water, wherein the reinforcing material comprises chopped fibers and modified polyhydroxyalkanoate.
2. The water-based epoxy mica iron oxide paint according to claim 1, characterized in that: The preparation method of the modified epoxy resin emulsion is as follows: pour propylene glycol methyl ether into epoxy resin particles, heat to 60-70° C., use a magnetic stirrer to stir until the epoxy resin is completely dissolved, pre-dissolve a nonionic surfactant in deionized water to prepare an emulsifier aqueous solution, slowly pour the propylene glycol methyl ether solution containing the resin into the emulsifier aqueous solution, and use a high-speed disperser to perform variable speed stirring to form an emulsion, add the pretreated silane, and after dispersion and emulsification are completed, cool the emulsion to room temperature, and continue stirring until the emulsion is stable.
3. The water-based epoxy mica iron oxide paint according to claim 2, characterized in that: The ratio of the epoxy resin particles, propylene glycol methyl ether and the emulsifier aqueous solution is 6:3:
1.
4. The water-based epoxy mica iron oxide paint according to claim 2, characterized in that: The silane pretreatment method is as follows: 1-5% of the weight of epoxy resin particles is mixed with ethanol water solution, the concentration of silane is 0.5%, and the pH value is adjusted to 4-6 at room temperature.
5. The water-based epoxy mica iron oxide paint according to claim 1, characterized in that: The ratio of the chopped fibers to the modified polyhydroxyalkanoate is 2-3:1, and the chopped fibers are modified hollow glass fibers.
6. The water-based epoxy mica iron oxide paint according to claim 5, characterized in that: The preparation method of the modified hollow glass fiber is as follows: In the drawing process of manufacturing glass fiber, gas is introduced to form a hollow structure to make hollow glass fiber. The hollow glass fiber is treated with hydrofluoric acid to corrode part of the surface to form a microporous structure. At the same time, the surface of the glass fiber is activated. The activated glass fiber is immersed in a polyethylene glycol solution, and a catalyst azobisisobutyronitrile is added to initiate a free radical polymerization reaction so that the polymer forms a graft layer directly on the fiber surface. After the reaction is completed, the glass fiber is washed with deionized water to remove unreacted monomers and by-products, and then dried in a vacuum oven to constant weight.
7. The water-based epoxy mica iron oxide paint according to claim 1, characterized in that: The preparation method of the modified polyhydroxyalkanoate is as follows: The polyhydroxyalkanoate particles are immersed in a 0.1M NaIO4 solution and treated at room temperature for 1-2 hours. After the oxidation treatment, the polyhydroxyalkanoate particles are washed with deionized water several times to remove residual NaIO4, and then dried in a vacuum oven to complete the activation of the polyhydroxyalkanoate particles. The activated polyhydroxyalkanoate particles are dispersed in a DCM organic solvent, PEG-NH2 and a catalyst DCC, as well as a small amount of NHS are added to help form a stable amide bond. Under nitrogen protection, the reaction mixture is placed under heating conditions of 40-50°C for reaction for 5-24 hours. After the reaction is completed, the grafted polyhydroxyalkanoate is separated by centrifugation and then washed with ethanol and water to remove unreacted PEG, DCC byproducts and other impurities. Finally, the product is dried under vacuum until the solvent is completely removed to obtain a modified polyhydroxyalkanoate.
8. The water-based epoxy mica iron oxide paint according to claim 7, characterized in that: The average particle size of the mica iron oxide pigment is less than 5 μm, and the purity is greater than 98%.
9. The water-based epoxy mica iron oxide paint according to claim 8, characterized in that: The auxiliary agent includes at least one of a defoaming agent, a preservative, a pH regulator, a thickener, and a wetting agent.
10. A method for producing a waterborne epoxy mica iron oxide paint as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Mix the modified waterborne epoxy resin emulsion and deionized water, dilute the modified waterborne epoxy resin emulsion, and mix the reinforcing material with deionized water for pre-dispersion, and mix the pre-dispersed reinforcing material with the diluted modified waterborne epoxy resin emulsion, use high-speed dispersing equipment to ensure uniform distribution, add mica iron oxide pigment and additives to continue mixing, add deionized water, and adjust the consistency of component A; Step 2: Mix the water-based phenolic amine curing agent, triethanolamine and an appropriate amount of deionized water, stir evenly and support component B for later use; Step 3: Mix component A and component B, stir evenly and then apply.
Citation Information
Cited By
Polysiloxane-fluorocarbon modified waterborne epoxy anticorrosive paint and preparation method thereof
CN120682702A