Low-temperature-resistant acrylic coating adhesive and preparation method thereof

By using raw materials such as methyl methacrylate, acrylic soft segment monomer and modified montmorillonite, combined with the complex cross-linking technology of persulfate initiator and zinc acetate, the problem of low temperature and acid-base conditions of acrylic coating glue has been solved. It significantly improves its low temperature resistance, acid and alkali resistance and bonding properties.

CN118755418AInactive Publication Date: 2024-10-11GUANGDONG ADVANCED REFRIGERATION TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411068989.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing acrylic coating adhesives perform poorly in terms of low temperature and acidity and alkalinity, and their bonding properties also need to be improved.

Method used

Using raw materials such as methyl methacrylate, acrylic soft segment monomer, emulsifier, modified montmorillonite, zinc acetate and sodium bicarbonate, the copolymerization reaction is carried out through the reaction of pre-emulsion and seed emulsion, combined with persulfate as the initiator. , and improve the cross-linking degree and dispersion of the polymer through the complex cross-linking of zinc acetate.

Benefits of technology

Significantly improves the low temperature resistance, acid and alkali resistance and bonding properties of the coating glue, and enhances its stability and adhesion in low temperature and corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980254540000031
    Figure BDA0004980254540000031
  • Figure BDA0004980254540000032
    Figure BDA0004980254540000032
  • Figure BDA0004980254540000111
    Figure BDA0004980254540000111
Patent Text Reader

Abstract

The invention relates to a low-temperature-resistant acrylic coating adhesive and a preparation method thereof, and belongs to the technical field of binders, the low-temperature-resistant acrylic coating adhesive comprises the following raw materials by weight: 20-50 parts of methyl methacrylate; the preparation method comprises the following steps: 1-6 parts of an acrylic acid soft segment monomer, 1-5 parts of an emulsifier, 0.1-1 part of persulfate, 1-5 parts of modified montmorillonite, 2-4 parts of zinc acetate, 0.05-1 part of sodium bicarbonate and 30-90 parts of deionized water; according to the invention, the acrylic acid soft segment monomer and the modified montmorillonite are added into the coating adhesive, and the acrylic acid soft segment monomer contains active hydroxyl, amino, carboxyl, flexible long-chain alkane and phosphate bonds, can participate in the curing reaction of an acrylate polymer, and also can be physically crosslinked with the modified montmorillonite; the overall crosslinking density of an acrylate polymer system is improved, the low temperature resistance of the coating adhesive is improved, and meanwhile, the cohesiveness and the acid and alkali resistance of the coating adhesive are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a low-temperature resistant acrylic coating adhesive and a preparation method thereof. Background Art

[0002] Acrylic resin is widely used in automotive and architectural coatings because of its good gloss retention, color retention, heat resistance, corrosion resistance and other properties. However, acrylic resin itself has the defects of becoming brittle at low temperatures and becoming sticky at high temperatures.

[0003] Chinese patent CN110643251A discloses a protective agent for facing stone based on fluorosilicone acrylic resin and a preparation method thereof. The protective agent is composed of the following raw material components by weight: 5-20 parts of fluorosilicone acrylic resin solution; 10-50 parts of silane coupling agent; 1-10 parts of low molecular weight terminal hydroxyl silicone oil; 20-85 parts of diluent, and 0.5-2 parts of catalyst. The invention has reasonable material cost, simple process, and is conducive to large-scale production. The prepared stone protective agent has good waterproof and oil-repellent effect, does not change the natural appearance and air permeability of the stone, and does not contain perfluorinated segments of 8 carbons or more, meeting environmental protection requirements. However, although the coating adhesive prepared by the invention improves its bonding performance, its low temperature resistance and acid and alkali resistance are poor, and its bonding performance also needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to provide to solve the following technical problems:

[0005] How to prepare low-temperature resistant acrylic coating adhesive with good acid and alkali resistance and high bonding performance.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A low-temperature resistant acrylic coating adhesive comprises the following raw materials in parts by weight: 20-50 parts of methyl methacrylate; 1-6 parts of acrylic soft segment monomer, 1-5 parts of emulsifier, 0.1-1 parts of persulfate, 1-5 parts of modified montmorillonite, 2-4 parts of zinc acetate, 0.05-1 parts of sodium bicarbonate and 30-90 parts of deionized water;

[0008] The preparation method of the low-temperature resistant acrylic coating adhesive comprises the following steps:

[0009] Step A1, add methyl methacrylate, acrylic acid soft segment monomer, emulsifier and 1 / 3 mass part of deionized water into a three-necked flask, stir at room temperature for 1-2 hours to obtain a pre-emulsion;

[0010] Pre-emulsification can avoid the phenomenon of excessive local concentration of emulsifier and monomer in the reaction materials, make the dispersion more uniform, the reaction more complete, and reduce the occurrence of gel, thus achieving controllable, efficient and convenient preparation and production;

[0011] Step A2, under nitrogen protection, add 1 / 10 mass parts of pre-emulsion, sodium bicarbonate and 1 / 2 mass parts of modified montmorillonite into a three-necked flask, heat to 70-85° C., dropwise add a persulfate aqueous solution prepared by 1 / 2 mass parts of persulfate and 1 / 3 mass parts of deionized water, reflux for 4-6 hours, and obtain a seed emulsion;

[0012] Step A3, adding the remaining pre-emulsion in step A1, the remaining modified montmorillonite and a persulfate aqueous solution prepared by 1 / 2 mass part of persulfate and 1 / 3 mass part of deionized water dropwise to the seed emulsion prepared in step A2 through two separate feed ports within 2-3.5 hours, then adding zinc acetate, ultrasonically dispersing for 1-2 hours, heat preservation for 0.1-2 hours, and then cooling to obtain a low-temperature resistant acrylic coating adhesive;

[0013] Using persulfate as an initiator, methyl methacrylate and acrylic acid soft segment monomer undergo free radical copolymerization. After the reaction is completed, zinc acetate is added to further increase the crosslinking degree of the polymer by ionic complex crosslinking with carboxylic acid.

[0014] Furthermore, the method for preparing the acrylic acid soft segment monomer comprises the following steps:

[0015] Step B1, add dimethyl phosphite, carbon tetrachloride and tetrahydrofuran into a three-necked flask, place in an ice bath, control the temperature at 0-2°C, add triethylamine and tris(hydroxymethyl)aminomethane, raise the temperature to 50-60°C, stir and react for 10-12h, filter with suction, and rotary evaporate the filtrate at 70°C to constant weight to obtain trihydroxyphosphate;

[0016] The dosage ratio of dimethyl phosphite, carbon tetrachloride, tetrahydrofuran and tris(hydroxymethyl)aminomethane is 40-45mL: 40-50mL: 40-45mL: 50-60mL. Using dimethyl phosphite and tris(hydroxymethyl)aminomethane as raw materials, a compound containing three hydroxyl groups, one secondary amine group and a phosphate group is obtained through Michael addition reaction to obtain trihydroxy phosphate, and the structural formula is as follows:

[0017]

[0018] Step B2, adding itaconic acid, p-toluenesulfonic acid, p-hydroxyanisole, trihydroxyphosphate and n-hexane into a three-necked flask, heating to reflux, stirring and reacting for 4-5 hours, after the reaction is completed, removing n-hexane by vacuum distillation, washing the distillation product with deionized water, and drying to obtain an acrylic acid soft segment monomer;

[0019] The structural formula of the acrylic acid soft segment monomer is as follows:

[0020]

[0021] The dosage ratio of itaconic acid, p-toluenesulfonic acid, p-hydroxyanisole, trihydroxyphosphate and n-hexane is 1-1.5g:0.015-0.04g:0.03-0.08g:2-2.5g:40-50mL. Itaconic acid and trihydroxyphosphate are used as raw materials, p-toluenesulfonic acid is used as a catalyst, and p-hydroxyanisole is used as an inhibitor. Through esterification reaction, an acrylic acid soft segment monomer is obtained. The acrylic acid soft segment monomer contains unsaturated double bonds, carboxyl groups, hydroxyl groups, phosphate groups and other groups.

[0022] Furthermore, the preparation method of the modified montmorillonite comprises the following steps:

[0023] Add sodium montmorillonite and deionized water into a three-necked flask, stir at a speed of 1000-1200rpm / min for 1-2h, then add dioctadecyl dimethyl ammonium bromide solution, continue stirring for 4-6h, heat to 60-70℃, stir for 9-11h, centrifuge and wash thoroughly until AgNO3 is free of Br - appear, dried at 70-80°C for 20-22h, and ground to obtain modified montmorillonite;

[0024] The dosage ratio of sodium montmorillonite, deionized water and dioctadecyl dimethyl ammonium bromide solution is 3-5g: 60-70mL: 60-70mL, and dioctadecyl dimethyl ammonium bromide is intercalated and adsorbed onto the sodium montmorillonite layer to improve its dispersion performance.

[0025] Furthermore, the emulsifier is one or more of sodium dodecyl sulfate, 2-acrylamide-2-methylpropane sulfonic acid or sodium alkyl vinyl sulfonate mixed in any ratio.

[0026] Beneficial effects of the present invention:

[0027] (1) In order to improve the low temperature resistance of the acrylic coating adhesive, the present invention adds modified montmorillonite and modifies the sodium montmorillonite by dioctadecyl dimethyl ammonium bromide. First, long-chain alkanes are introduced into the sodium montmorillonite. The long-chain alkanes have a lower glass transition temperature and enhance the low temperature resistance of the acrylic coating adhesive. Second, the interlayer spacing of the sodium montmorillonite is enlarged by the modification. The enlarged interlayer spacing not only creates a spatial environment for the insertion of the acrylic soft segment monomer, but also greatly reduces the van der Waals force between the layers. In this way, the dispersibility and compatibility of the sodium montmorillonite in the coating adhesive are increased, and the improvement of the low temperature resistance of the coating adhesive by the modified montmorillonite is further enhanced.

[0028] (2) In order to improve the acid and alkali resistance of the acrylic coating adhesive, the present invention adds acrylic soft segment monomers and modified montmorillonite. The amino groups on the phosphate ester in the acrylic soft segment monomer and the dihydroxyl groups on the flexible chain segment can form a stable protective film between the coating and the metal substrate to prevent the horizontal diffusion of the corrosive medium, slow down the corrosion and peeling of the coating defects, and improve the acid and alkali resistance of the coating adhesive. At the same time, the oxygen atoms on the phosphate ester have strong electronegativity, the zinc ions in the cross-linking agent have positive charge, and the crystal layers of the modified montmorillonite have negative charge and ammonium ions on the layers. Therefore, the acrylic soft segment monomer and the cross-linking agent can have a strong interaction with the modified montmorillonite. In addition, the hydroxyl groups in the acrylic soft segment monomer can form hydrogen bonds with the trace water remaining on the surface of the modified montmorillonite, so that the soft segment structure and the cross-linking agent can be intercalated into the modified montmorillonite layers and physically cross-linked with the modified montmorillonite sheets to form a network, further enhancing the acid and alkali resistance.

[0029] (3) In order to improve the bonding performance of the acrylic coating adhesive, the present invention introduces an acrylic soft segment monomer into the acrylic coating adhesive. The acrylic soft segment monomer contains hydrophilic hydroxyl, amino and carboxyl groups. These active groups have strong hydrophilicity and can produce hydrogen bonds with trace moisture on the surface of the substrate, thereby significantly enhancing the bonding performance of the coating adhesive. At the same time, the flexible long-chain alkanes in the acrylic soft segment monomer can also enhance the movement of the polymer macromolecular chain segments in the coating adhesive, thereby enhancing the bonding performance of the acrylic coating adhesive. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] This embodiment provides a method for preparing an acrylic acid soft segment monomer, comprising the following steps:

[0033] Step B1, add 40 mL of dimethyl phosphite, 40 mL of carbon tetrachloride and 40 mL of tetrahydrofuran into a three-necked flask, place in an ice bath, control the temperature at 0°C, add 50 mL of tris(hydroxymethyl)aminomethane, raise the temperature to 50°C, stir and react for 10 hours, filter with suction, and rotary evaporate the filtrate at 70°C to constant weight to obtain trihydroxyphosphate;

[0034] Step B2, add 1g of itaconic acid, 0.015g of p-toluenesulfonic acid, 0.03g of p-hydroxyanisole, 2g of trihydroxyphosphate and 40mL of n-hexane into a three-necked flask, heat to reflux, stir and react for 4h. After the reaction is completed, remove the n-hexane by vacuum distillation, wash the distillation product with deionized water, and dry to obtain an acrylic acid soft segment monomer.

[0035] Example 2

[0036] This embodiment provides a method for preparing an acrylic acid soft segment monomer, comprising the following steps:

[0037] Step B1, add 42.5 mL of dimethyl phosphite, 45 mL of carbon tetrachloride and 42.5 mL of tetrahydrofuran into a three-necked flask, place in an ice bath, control the temperature at 1°C, add 55 mL of tris(hydroxymethyl)aminomethane, stir and react at room temperature for 11 h, filter with suction, and evaporate the filtrate at 70°C to constant weight to obtain trihydroxyphosphate;

[0038] Step B2, add 1.25g of itaconic acid, 0.02g of p-toluenesulfonic acid, 0.055g of p-hydroxyanisole, 2.25g of trihydroxyphosphate and 45mL of n-hexane into a three-necked flask, heat to reflux, stir and react for 4.5h. After the reaction is completed, remove the n-hexane by vacuum distillation, wash the distillation product with deionized water, and dry to obtain an acrylic acid soft segment monomer.

[0039] Example 3

[0040] This embodiment provides a method for preparing an acrylic acid soft segment monomer, comprising the following steps:

[0041] Step B1, add 45 mL of dimethyl phosphite, 50 mL of carbon tetrachloride and 45 mL of tetrahydrofuran into a three-necked flask, place in an ice bath, control the temperature at 2°C, add 60 mL of tris(hydroxymethyl)aminomethane, stir and react at room temperature for 12 h, filter with suction, and evaporate the filtrate at 70°C to constant weight to obtain trihydroxyphosphate;

[0042] Step B2, add 1.5g of itaconic acid, 0.04g of p-toluenesulfonic acid, 0.08g of p-hydroxyanisole, 2.5g of trihydroxyphosphate and 50mL of n-hexane into a three-necked flask, heat to reflux, stir and react for 5h. After the reaction is completed, remove the n-hexane by vacuum distillation, wash the distillation product with deionized water, and dry to obtain an acrylic acid soft segment monomer.

[0043] Example 4

[0044] This embodiment provides a method for preparing modified montmorillonite, comprising the following steps:

[0045] Add 3g of sodium montmorillonite and 60mL of deionized water into a three-necked flask, stir at 1000rpm / min for 1h, then add 60mL of dioctadecyl dimethyl ammonium bromide solution, continue stirring for 4h, heat to 60℃, stir for 9h, centrifuge and wash thoroughly until AgNO3 is free of Br - It appeared, dried at 70°C for 20h, and ground to obtain modified montmorillonite, wherein dioctadecyl dimethyl ammonium bromide is prepared by mixing hexadecyl trimethyl ammonium bromide and 15wt% hydrochloric acid aqueous solution in a dosage ratio of 10g:60mL.

[0046] Example 5

[0047] This embodiment provides a method for preparing modified montmorillonite, comprising the following steps:

[0048] 4 g of sodium montmorillonite and 65 mL of deionized water were added to a three-necked flask, stirred at 1100 rpm / min for 1.5 h, then 65 mL of dioctadecyl dimethyl ammonium bromide solution was added, and stirring continued for 5 h. The temperature was raised to 65 °C, stirred for 10 h, centrifuged, and washed thoroughly until AgNO3 was detected to be free of Br. - It appeared, dried at 75° C. for 21 h, and ground to obtain modified montmorillonite, wherein dioctadecyl dimethyl ammonium bromide was prepared by mixing hexadecyl trimethyl ammonium bromide and 15 wt % hydrochloric acid aqueous solution in a dosage ratio of 12.5 g: 65 mL.

[0049] Example 6

[0050] This embodiment provides a method for preparing modified montmorillonite, comprising the following steps:

[0051] Add 5g of sodium montmorillonite and 70mL of deionized water into a three-necked flask, stir at 1200rpm / min for 2h, then add 70mL of dioctadecyl dimethyl ammonium bromide solution, continue stirring for 6h, heat to 70℃, stir for 11h, centrifuge and wash thoroughly until AgNO3 is free of Br - It appeared, dried at 80 °C for 22 h, and ground to obtain modified montmorillonite.

[0052] Example 7

[0053] This embodiment provides a low-temperature resistant acrylic coating adhesive, comprising the following raw materials in parts by weight: 20 parts of methyl methacrylate, 1 part of acrylic soft segment monomer prepared in Example 1, 1 part of sodium dodecyl sulfate, 0.1 part of ammonium persulfate, 1 part of modified montmorillonite prepared in Example 4, 2 parts of zinc acetate, 0.05 parts of sodium bicarbonate and 30 parts of deionized water;

[0054] The preparation method of the low-temperature resistant acrylic coating adhesive comprises the following steps:

[0055] Step A1, add 20 parts of methyl methacrylate, 1 part of acrylic acid soft segment monomer, 1 part of sodium dodecyl sulfate and 10 parts of deionized water into a three-necked flask, and stir at room temperature for 1 hour to obtain a pre-emulsion;

[0056] Step A2, under nitrogen protection, add 1 / 10 mass part of the pre-emulsion, 0.05 parts of sodium bicarbonate and 0.5 parts of modified montmorillonite into a three-necked flask, heat to 70° C., dropwise add an aqueous solution of ammonium persulfate prepared by 0.05 parts of ammonium persulfate and 10 parts of deionized water, reflux for 4 hours to obtain a seed emulsion;

[0057] Step A3, the remaining pre-emulsion in step A1, 0.5 parts of modified montmorillonite and an ammonium persulfate solution prepared by 0.05 parts of ammonium persulfate and 10 parts of deionized water are added dropwise to the seed emulsion prepared in step A2 through two separate feed ports within 2 hours, and then 2 parts of zinc acetate are added, ultrasonic dispersion is performed for 1 hour, and the heat preservation is terminated after 0.1 hour, and cooling is performed to obtain a low-temperature resistant acrylic coating adhesive.

[0058] Example 8

[0059] This embodiment provides a low-temperature resistant acrylic coating adhesive, comprising the following raw materials in parts by weight: 35 parts of methyl methacrylate, 3.5 parts of acrylic soft segment monomer prepared in Example 2, 3 parts of 2-acrylamide-2-methylpropanesulfonic acid, 0.55 parts of sodium persulfate, 3 parts of modified montmorillonite prepared in Example 5, 3 parts of zinc acetate, 0.55 parts of sodium bicarbonate and 60 parts of deionized water;

[0060] The preparation method of the low-temperature resistant acrylic coating adhesive comprises the following steps:

[0061] Step A1, add 35 parts of methyl methacrylate, 3.5 parts of acrylic acid soft segment monomer, 3 parts of 2-acrylamide-2-methylpropanesulfonic acid and 20 parts of deionized water into a three-necked flask, stir at room temperature for 1.5 hours to obtain a pre-emulsion;

[0062] Step A2, under nitrogen protection, add 1 / 10 mass parts of the pre-emulsion, 0.55 parts of sodium bicarbonate and 1.5 parts of modified montmorillonite into a three-necked flask, heat to 78° C., dropwise add a sodium persulfate aqueous solution prepared by 0.25 parts of sodium persulfate and 30 parts of deionized water, reflux for 5 hours, and obtain a seed emulsion;

[0063] Step A3, the remaining pre-emulsion in step A1, 1.5 parts of modified montmorillonite and a sodium persulfate aqueous solution prepared by 0.30 parts of sodium persulfate and 30 parts of deionized water are added dropwise to the seed emulsion prepared in step A2 through two separate feed ports within 3 hours, and then 3 parts of zinc acetate are added, ultrasonic dispersion is performed for 1.5 hours, and the heat preservation is terminated after 1 hour, and cooling is performed to obtain a low-temperature resistant acrylic coating adhesive.

[0064] Example 9

[0065] This embodiment provides a low-temperature resistant acrylic coating adhesive, comprising the following raw materials in parts by weight: 50 parts of methyl methacrylate, 6 parts of acrylic soft segment monomer prepared in Example 3, 5 parts of sodium alkyl vinyl sulfonate, 1 part of potassium persulfate, 5 parts of modified montmorillonite prepared in Example 6, 4 parts of zinc acetate, 1 part of sodium bicarbonate and 90 parts of deionized water;

[0066] The preparation method of the low-temperature resistant acrylic coating adhesive comprises the following steps:

[0067] Step A1, add 50 parts of methyl methacrylate, 6 parts of acrylic acid soft segment monomer, 5 parts of sodium alkyl vinyl sulfonate and 30 parts of deionized water into a three-necked flask, stir at room temperature for 2 hours to obtain a pre-emulsion;

[0068] Step A2, under nitrogen protection, add 1 / 10 mass part of the pre-emulsion, 1 part of sodium bicarbonate and 2.5 parts of modified montmorillonite into a three-necked flask, heat to 85° C., dropwise add a potassium persulfate aqueous solution prepared by 0.45 parts of potassium persulfate and 30 parts of deionized water, reflux for 6 hours, and obtain a seed emulsion;

[0069] Step A3, the remaining pre-emulsion in step A1, 2.5 parts of modified montmorillonite and a potassium persulfate aqueous solution prepared by 0.55 parts of potassium persulfate and 30 parts of deionized water are added dropwise to the seed emulsion prepared in step A2 through two separate feed ports within 3.5 hours, and then 4 parts of zinc acetate are added, ultrasonic dispersion is performed for 2 hours, and heat preservation is terminated after 2 hours, and cooling is performed to obtain a low-temperature resistant acrylic coating adhesive.

[0070] Comparative Example 1

[0071] The dimethyl phosphite in Example 1 was removed, and the other raw materials and preparation process remained unchanged.

[0072] Comparative Example 2

[0073] The itaconic acid in Example 2 was removed, and the other raw materials and preparation process remained unchanged.

[0074] Comparative Example 3

[0075] The dioctadecyl dimethyl ammonium bromide solution in Example 4 was removed, and the remaining raw materials and preparation process remained unchanged.

[0076] Comparative Example 4

[0077] The acrylic acid soft segment monomer in Example 7 was replaced by the substance prepared in Comparative Example 1, and the other raw materials and preparation process remained unchanged.

[0078] Comparative Example 5

[0079] The acrylic acid soft segment monomer in Example 8 was replaced by the substance prepared in Comparative Example 2, and the other raw materials and preparation process remained unchanged.

[0080] Comparative Example 6

[0081] The modified montmorillonite in Example 9 was replaced by the material prepared in Comparative Example 3, and the other raw materials and preparation process remained unchanged.

[0082] Comparative Example 7

[0083] The acrylic acid soft segment monomer in Example 9 was removed, and the other raw materials and preparation process remained unchanged.

[0084] Comparative Example 8

[0085] The modified montmorillonite in Example 9 was removed, and the other raw materials and preparation process remained unchanged.

[0086] Performance Testing

[0087] 1. The low-temperature resistant acrylic coating adhesive prepared in Examples 7-9 and Comparative Examples 4-8 was coated on a 30 μm thick and 25 mm wide polyethylene terephthalate (PET) strip using a wire coater to obtain a wet adhesive layer with a thickness of 40 μm. The coated sample was placed in an oven at 90°C and dried for 20 minutes to remove the residual liquid in the emulsion, and then dried in a vacuum oven at 105°C for 5 minutes to complete the curing and internal self-crosslinking of the adhesive layer. The PET coated with the acrylic coating adhesive on one side was attached with release paper to prepare a test sample.

[0088] The test samples prepared in the above-mentioned examples 7-9 and comparative examples 4-8 were respectively tested for initial adhesion and 180° peel strength at low temperature. The specific test results are shown in Table 1. The specific test method is as follows:

[0089] (1) Initial Adhesion The test was conducted in accordance with GB / T4852-2002 Test Method for Initial Adhesion of Acrylic Coated Adhesive Tapes (Rolling Ball Method) at an ambient temperature of 0°C using a pressure-sensitive tape initial adhesion performance tester.

[0090] (2) 180° peel strength was measured according to the standard "ASTM D3330 Peel Strength of Pressure-Sensitive Tapes", and the initial adhesion (20 min) and the lasting adhesion (24 h) of the test sample were measured at 0°C. The test was performed using a tape retention tester.

[0091] 2. Acid and alkali resistance test

[0092] The low-temperature resistant acrylic coating glue prepared in Examples 7-9 and Comparative Examples 4-8 was rolled back and forth 3 times with a 2kg roller and adhered to a clean glass plate. The glass plate was placed in a strong acid (pH=2) or a strong base (pH=13) and soaked for 1 hour. Then, it was taken out and rinsed with clean water. After drying at room temperature, the protective film sample was peeled off the glass plate, and the contamination on the surface of the glass plate after the protective film sample was peeled off was observed under a strong light in a dark room.

[0093] The specific test results are shown in Table 1:

[0094] Table 1

[0095]

[0096] Note: ○ indicates no pollution and no residual glue; △ indicates slight pollution, with white mist or crystal spots on the surface of the glass plate; ◇ indicates moderate to severe pollution, with large areas of white mist or crystal spots on the surface of the glass plate.

[0097] It can be seen from Table 1 that, compared with Comparative Examples 4-8, the low-temperature resistant acrylic coating adhesive prepared in Examples 7-9 has better low-temperature resistance, acid and alkali resistance and bonding performance.

[0098] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0099] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A low temperature resistant acrylic coating adhesive, Features: A low-temperature resistant acrylic coating adhesive comprises the following raw materials in parts by weight: 20-50 parts of methyl methacrylate; 1-6 parts of acrylic soft segment monomer, 1-5 parts of emulsifier, 0.1-1 parts of persulfate, 1-5 parts of modified montmorillonite, 2-4 parts of zinc acetate, 0.05-1 parts of sodium bicarbonate and 30-90 parts of deionized water; The preparation method of the acrylic acid soft segment monomer comprises the following steps: Step B1, add dimethyl phosphite, carbon tetrachloride and tetrahydrofuran into a three-necked flask, place in an ice bath, control the temperature at 0-2°C, add tris(hydroxymethyl)aminomethane, raise the temperature to 50-60°C, stir and react for 10-12h, filter with suction, and rotary evaporate the filtrate at 70°C to constant weight to obtain trihydroxy phosphate; Step B2, add itaconic acid, p-toluenesulfonic acid, p-hydroxyanisole, trihydroxyphosphate and n-hexane into a three-necked flask, heat to reflux, stir and react for 4-5 hours. After the reaction is completed, remove the n-hexane by vacuum distillation, wash the distillation product with deionized water, and dry to obtain an acrylic acid soft segment monomer.

2. A low temperature resistant acrylic coating adhesive according to claim 1, It is characterized in that The usage ratio of dimethyl phosphite, carbon tetrachloride, tetrahydrofuran and tris(hydroxymethyl)aminomethane is 40-45mL:40-50mL:40-45mL:50-60mL.

3. A low temperature resistant acrylic coating adhesive according to claim 1, It is characterized in that The dosage ratio of itaconic acid, p-toluenesulfonic acid, p-hydroxyanisole, trihydroxyphosphate and n-hexane is 1-1.5 g: 0.015-0.04 g: 0.03-0.08 g: 2-2.5 g: 40-50 mL.

4. The low temperature resistant acrylic coating adhesive according to claim 1, It is characterized in that The preparation method of modified montmorillonite comprises the following steps: Add sodium montmorillonite and deionized water into a three-necked flask, stir for 1-2 hours at a speed of 1000-1200 rpm / min, then add dioctadecyl dimethyl ammonium bromide solution, continue stirring for 4-6 hours, heat to 60-70 ° C, stir for 9-11 hours, centrifuge and wash thoroughly until AgNO 3 Detection of no Br - It appeared, dried at 70-80°C for 20-22h, and ground to obtain modified montmorillonite.

5. A low temperature resistant acrylic coating adhesive according to claim 4, It is characterized in that The dosage ratio of sodium montmorillonite, deionized water and dioctadecyl dimethyl ammonium bromide is 3-5g:60-70mL:60-70mL.

6. A low temperature resistant acrylic coating adhesive according to claim 4, It is characterized in that The dioctadecyl dimethyl ammonium bromide is prepared by mixing hexadecyl trimethyl ammonium bromide and a 15 wt% hydrochloric acid aqueous solution in a dosage ratio of 10-15 g: 60-70 mL.

7. The low temperature resistant acrylic coating adhesive according to claim 1, It is characterized in that The persulfate is a mixture of one or more of ammonium persulfate, sodium persulfate, potassium persulfate in any ratio.

8. A method for preparing a low-temperature resistant acrylic coating adhesive according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Step A1, add methyl methacrylate, acrylic acid soft segment monomer, emulsifier and 1 / 3 mass part of deionized water into a three-necked flask, and stir at room temperature for 1-2 hours to obtain a pre-emulsion; Step A2, under nitrogen protection, add 1 / 10 mass parts of pre-emulsion, sodium bicarbonate and 1 / 2 mass parts of modified montmorillonite into a three-necked flask, heat to 70-85° C., dropwise add a persulfate aqueous solution prepared by 1 / 2 mass parts of persulfate and 1 / 3 mass parts of deionized water, reflux for 4-6 hours, and obtain a seed emulsion; Step A3, adding the remaining pre-emulsion in step A1, the remaining mass parts of modified montmorillonite and a persulfate aqueous solution prepared by 1 / 2 mass parts of persulfate and 1 / 3 mass parts of deionized water dropwise to the seed emulsion prepared in step A2 through two separate feed ports within 2-3.5 hours, then adding zinc acetate, ultrasonically dispersing for 1-2 hours, heat preservation for 0.1-2 hours, and cooling to obtain Claim to low temperature resistant acrylic coating glue.

Citation Information

Patent Citations

  • Finishing type stone protection agent based on fluorosilicone acrylic resin, and preparation method thereof

    CN110643251A