Soil solidification material based on primary enzyme modified nano-particles cooperating with solid waste

Through the synergistic use of native enzyme-modified nanoparticles and industrial solid waste, the problem of insufficient strength and water stability of soil solidification materials is solved, efficient and environmentally friendly soil solidification materials are provided, and the compactness and load-bearing capacity of the soil are significantly improved. Capacity, suitable for processing industrial waste and construction waste.

CN118755481APending Publication Date: 2024-10-11CHONGQING UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410838683.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing soil solidification materials have deficiencies in strength and water stability, especially for clay and organic soil with high plasticity index. The cement production process pollutes the environment and endangers human health.

Method used

Soil solidification materials based on native enzyme-modified nanoparticles and solid waste are used to form an efficient solidifying agent by combining native enzymes with nanomaterials and industrial solid waste. The native enzyme extraction process includes the preparation of native enzyme crude enzyme solution, salt Analysis and ion exchange chromatography, nanomaterials such as nano-SiO2, nano-Al2O3 are used to improve the bonding and polymerization reactions between soil particles.

Benefits of technology

Significantly improve the compactness and load-bearing capacity of the soil, reduce the water absorption capacity of soil particles, form a waterproof layer, enhance the overall strength of the soil, and solve the problems of environmental pollution and resource waste of solid waste, providing non-toxic , environmentally friendly curing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755481A_ABST
    Figure CN118755481A_ABST
Patent Text Reader

Abstract

The invention discloses a soil solidification material based on primary enzyme modified nano-particles cooperating with solid waste, the soil solidification material comprises the following components in parts by weight: 8-12 parts of industrial solid waste, 2-6 parts of an exciting agent, 0-7 parts of primary enzyme and 0-2 parts of a nano-material, and the invention relates to the technical field of soil solidification agents. The primary enzyme and the nano-particles synergistically solidify the soil body, the primary enzyme and the nano-particles can play a role in solidification, meanwhile, the primary enzyme can modify the nano-particles, the dispersity of the nano-particles is improved, the filling effect is improved, and due to the fact that both the primary enzyme and the nano-particles can play a role in promoting a polymerization reaction in the soil body, the soil body can be well solidified. After the nano-particles are modified by the primary enzyme, the uniformly distributed nano-particles can more fully exert the seed crystal nucleation effect of the nano-particles, the polymerization reaction is accelerated, and the overall strength of the soil body is higher due to the increase of a gelatinization product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of soil solidifying agents, in particular to a soil solidifying material based on native enzyme-modified nanoparticles in collaboration with solid waste. Background Art

[0002] At present, soil solidification usually adopts physical solidification, chemical solidification, heat treatment solidification, grouting solidification and other methods. Chemical solidification is the most commonly used method of soil solidification. After adding the solidification material to the soil, physical and chemical reactions can occur to solidify the soil particles. It has the advantages of rapid solidification, small amount of use, local materials and reduced engineering costs. It is widely used in various engineering fields.

[0003] In the early days, lime and cement were mainly used to solidify soil. Although they have good strength, lime-solidified soil has poor water stability, and cement-solidified soil has large shrinkage and is prone to cracking. For clay and organic soil with high plasticity index, cement and lime have poor solidification effects and may even fail. At the same time, the cement production process pollutes the environment and harms human health.

[0004] In view of this, researchers at home and abroad have developed a series of new green and environmentally friendly soil solidification materials, such as bio-enzyme soil solidifiers, ionic soil solidifiers, composite soil solidifiers, etc. However, the new soil solidifiers still have disadvantages such as low strength, poor water stability, and large temperature shrinkage and dry shrinkage. It is still necessary to research and develop soil solidification materials with better curing effects. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a soil solidification material based on native enzyme-modified nanoparticles in collaboration with solid waste, which solves the above-mentioned problems.

[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: a soil solidification material based on native enzyme-modified nanoparticles and solid waste, the soil solidification material comprising:

[0007] 8-12 parts of industrial solid waste, 2-6 parts of stimulant, 0-7 parts of native enzyme, and 0-2 parts of nanomaterial.

[0008] Preferably, the weight components of the soil solidification material are: 8-12 parts of industrial solid waste, 2-6 parts of activator, 0-7 parts of native enzyme, and 0-2 parts of nanomaterial.

[0009] Preferably, the industrial solid waste is selected from one or a mixture of two or more of fly ash, slag, silicon powder, steel slag, carbide slag and quicklime.

[0010] Preferably, the activator is selected from one or a mixture of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate, and sodium silicate.

[0011] Preferably, the native enzyme is obtained by a protease extraction process from Gramineae plants and insects.

[0012] Preferably, the extraction process of the native enzyme comprises the following steps:

[0013] (1) Preparing crude enzyme solution of native enzyme: washing grass plants such as barley and insects such as ants obtained from nature, grinding and crushing plants in a mortar with a pestle, crushing animals with a meat grinder, collecting the crushed and filtered liquid of the plants and animals, and homogenizing them with a homogenizer, mixing the slurry with a buffer solution at a ratio of 1:6, and extracting at a pH of 4 to 6 and a temperature of 25 to 35°C for 2 to 5 hours, and obtaining crude enzyme solution of native enzyme after centrifugation;

[0014] (2) Salting out: Add the crude enzyme solution to a 60-80% ammonium sulfate solution, let stand at 4°C for 48-72 hours, centrifuge, take the supernatant, then add buffer, and dialyze for 12-24 hours. Perform salting out for at least 2-4 times;

[0015] (3) Ion exchange chromatography: The enzyme solution after salting out is loaded onto a DEAE ion exchange column, the pH of the buffer is controlled to 7, the flow rate is 1-3 mL / min, and then eluted with 0.4-0.6 mol / L NaCl in Tris-HCl. After elution, the native enzyme solution purified by ion exchange chromatography can be obtained.

[0016] Preferably, the nano material is selected from one or a mixture of two or more of nano-SiO2, nano-Al2O3, and nano-CaCO3.

[0017] The method for using the soil solidification material based on native enzyme modified nanoparticles and solid waste comprises the following steps: 1) drying the soil retrieved on site to obtain dry soil material, and rolling it through a 2 mm sieve; 2) diluting the native enzyme with water at a volume ratio of 1:500-1:1500; 3) mixing the diluted native enzyme with industrial solid waste, an activator and nanomaterials to prepare a soil solidifier; 4) uniformly mixing the soil solidifier, water and the soil to be solidified in a certain proportion.

[0018] Beneficial Effects

[0019] The present invention provides a soil solidification material based on native enzyme-modified nanoparticles in collaboration with solid waste. Compared with the prior art, it has the following beneficial effects:

[0020] The soil solidification material based on native enzyme-modified nanoparticles and solid waste has simple and convenient extraction of native enzymes. The native enzymes can reduce the thickness of the water film and enhance the adhesion between soil particles through ion exchange. They can also combine with organic macromolecules in the soil and adsorb on the surface of soil particles. All of the above reduce the water absorption capacity of soil particles and have a shielding effect on water to form a waterproof soil layer. The surfactant in the native enzymes can also reduce the surface tension of water and play a wetting role. Under the action of external force, the soil is easier to compact, and the density and bearing capacity of the soil are improved. When the native enzyme and nanoparticles in the present invention synergistically solidify the soil, the two can not only play their own solidification effect, but also the native enzyme can modify the nanoparticles to improve the dispersibility of the nanoparticles, that is, the surfactant in the native enzyme can be adsorbed on the surface of the nanoparticles, improve the hydrophobicity of the nanoparticles, make them more evenly distributed in the soil, improve the filling effect, and because both the native enzyme and the nanoparticles can promote the polymerization reaction in the soil, after the native enzyme modifies the nanoparticles, the evenly distributed nanoparticles can more fully play their "seed nucleation" effect, accelerate the polymerization reaction, and the increase of the gelled product makes the overall strength of the soil higher. The native enzyme and nanomaterial in the present invention are a non-toxic, environmentally friendly and pollution-free solidification material, which can achieve efficient solidification and significantly improve soil density. It can be widely used in the disposal of solid waste, such as the treatment of industrial waste residues, construction waste, etc., which can not only improve the strength of the soil, but also solve the pollution of solid waste to the environment and the waste of resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is the unconfined compressive strength diagram of Examples 1-8 of the present invention at 7d and 28d;

[0022] Figure 2 It is a curve diagram of unconfined compressive strength variation with time of Examples 1-8 and Comparative Examples 1-6 of the present invention;

[0023] Figure 3 It is the XRD phase analysis diagram of Shanghai soft soil in Examples 1-8 and Comparative Examples 1-6 of the present invention;

[0024] Figure 4 It is a graph showing the surface tension test results of the native enzyme solution of the present invention. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 5 parts of fly ash and 5 parts of slag; the activator is a mixture of 2 parts of sodium silicate and 2 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0028] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0029] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 22:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d (seventh day) and 28d (twenty-eighth day), and the results were: 7d compressive strength was 5.75MPa, and 28d compressive strength was 7.78MPa.

[0030] Example 2

[0031] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 3 parts of fly ash and 7 parts of slag; the activator is a mixture of 2 parts of sodium silicate and 2 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0032] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0033] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 22:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 9.01MPa, and 28d compressive strength was 12.17MPa.

[0034] Example 3

[0035] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 1 part of fly ash and 9 parts of slag; the activator is a mixture of 2 parts of sodium silicate and 2 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0036] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0037] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 22:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 9.92MPa, and 28d compressive strength was 12.86MPa.

[0038] Example 4

[0039] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 3 parts of fly ash and 7 parts of slag; the activator is a mixture of 3 parts of sodium silicate and 1 part of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0040] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0041] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 22:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 9.56MPa, and 28d compressive strength was 12.41MPa.

[0042] Example 5

[0043] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 3 parts of fly ash and 7 parts of slag; the activator is a mixture of 1 part of sodium silicate and 3 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0044] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0045] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 22:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 7.21MPa, and 28d compressive strength was 11.12MPa.

[0046] Example 6

[0047] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 10 parts of industrial solid waste, 6 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 3 parts of fly ash and 7 parts of slag; the activator is a mixture of 3 parts of sodium silicate and 3 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0048] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0049] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 24:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 7.55MPa, and 28d compressive strength was 9.17MPa.

[0050] Example 7

[0051] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 8 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 2.4 parts of fly ash and 5.6 parts of slag; the activator is a mixture of 2 parts of sodium silicate and 2 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0052] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0053] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 20:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 7.87MPa, and 28d compressive strength was 10.69MPa.

[0054] Example 8

[0055] In this embodiment, the soil solidification material based on native enzyme modified nanoparticles and solid waste includes the following components in mass ratio: 12 parts of industrial solid waste, 4 parts of activator, 7 parts of native enzyme, and 1 part of nanomaterial. Among them, the industrial solid waste is a mixture of 3.6 parts of fly ash and 8.4 parts of slag; the activator is a mixture of 2 parts of sodium silicate and 2 parts of sodium hydroxide; the native enzyme is diluted with water at a ratio of 1:1000; the nanomaterial is 1 part of nano-SiO2, and the specific surface area of ​​nano-SiO2 is 250±30m 2 / g, and the average particle size is 30nm. The above components are uniformly mixed to obtain a soil stabilizer.

[0056] The Shanghai soft soil retrieved from the site was placed in a constant temperature drying box and dried at 65°C for two days. The dried soft soil was crushed and passed through a 2mm sieve, and the sieved dry soft soil was taken for later use.

[0057] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 24:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 9.57MPa, and 28d compressive strength was 12.91MPa.

[0058] Comparative Example 1

[0059] Compared with Example 1, it does not contain nano-SiO2, and the rest of the parts are the same.

[0060] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 21:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 4.36MPa, and 28d compressive strength was 6.31MPa.

[0061] Comparative Example 2

[0062] Relative to Example 2, the native enzyme is not contained, and the rest are the same.

[0063] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 15:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 4.59MPa, and 28d compressive strength was 8.02MPa.

[0064] Comparative Example 3

[0065] Compared with Example 3, the amount of nano-SiO2 used is 0.2 parts, and the rest is the same.

[0066] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 21.2:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 5.06MPa, and 28d compressive strength was 9.75MPa.

[0067] Comparative Example 4

[0068] Compared with Example 4, the amount of native enzyme used is 3 parts, and the rest is the same.

[0069] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 18:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 5.21MPa, and 28d compressive strength was 9.95MPa.

[0070] Comparative Example 5

[0071] Compared with Example 5, the amount of the activator used is 2 parts, that is, the activator is a mixture of 0.5 parts of sodium silicate and 1.5 parts of sodium hydroxide, and the rest are the same.

[0072] The soil stabilizer, water and the soft soil to be solidified were mixed in a weight ratio of 20:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the "Standard for Geotechnical Test Methods" (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 5.04MPa, and 28d compressive strength was 9.12MPa.

[0073] Comparative Example 6

[0074] With respect to all the embodiments, only 14 parts of cement were added, and no other solidifying materials were added, namely, 0 parts of industrial solid waste, 0 parts of activator, 0 parts of native enzyme, and 0 parts of nanomaterial.

[0075] Cement, water and soft soil to be solidified were mixed in a weight ratio of 14:18:100, and samples with a height of 80 mm and a diameter of 39.1 mm were prepared according to the provisions of the Geotechnical Test Method Standard (GB / T50123-2019). The samples were cured in a curing box at a temperature of 20°C and a humidity of 90% to different ages and then tested for unconfined compressive strength. Three parallel samples were prepared in each group for testing, and the test results were averaged. The unconfined compressive strength was tested at 7d and 28d, and the results were: 7d compressive strength was 4.01MPa, and 28d compressive strength was 4.32MPa.

[0076] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0077] The unconfined compressive strength of Examples 1 to 8 at 7d and 28d is as follows: Figure 1 As shown, the unconfined compressive strength variation curves of Examples 1-8 and Comparative Examples 1-6 over time are as follows Figure 2 As shown, the XRD phase analysis of Shanghai soft soil in Examples 1-8 and Comparative Examples 1-6 is as follows Figure 3 As shown, the material composition and element content of Shanghai soft soil in Examples 1-8 and Comparative Examples 1-6 are shown in Table 1:

[0078]

[0079]

[0080] Table 1 Material composition and element content of Shanghai soft soil The basic physical parameters of Shanghai soft soil in Examples 1-8 and Comparative Examples 1-6 are shown in Table 2:

[0081]

[0082] Table 2 Basic physical parameters of Shanghai soft soil

[0083] At the same time, the surface tension of the native enzyme solution obtained by the present invention was tested by using a contact angle measuring instrument to perform a hanging drop method to test the surface tension. The test results are as follows: Figure 4 As shown, it can be seen that the native enzyme can significantly reduce the surface tension of water.

[0084] It can be seen from Examples 1-8 and Comparative Examples 1-6 that the soil solidification material provided in the present invention can effectively improve the density and bearing capacity of the soil body compared with traditional cement. This is because the native enzyme provided in the present invention can reduce the thickness of the water film and enhance the bonding between soil particles through ion exchange, and can also combine with organic macromolecules in the soil and adsorb on the surface of soil particles, all of which reduce the water absorption capacity of soil particles and have a shielding effect on water to form a waterproof soil layer. The surfactant in the native enzyme can also reduce the surface tension of water and play a wetting role. Under the action of external force, the soil body is easier to compact, and the density and bearing capacity of the soil body are improved. At the same time, the nanoparticles provided have the characteristics of small particle size (<100μm), large specific surface area, large surface energy, etc., and a structural aggregation effect is generated by filling the gaps between soil particles, thereby making the soil structure more compact. It can be seen from Example 2 and Comparative Example 2 that the soil bearing capacity when only nanoparticles are added is significantly less than the soil bearing capacity when nanoparticles and native enzymes are added at the same time. This is because the van der Waals force, electrostatic force and other forces between nanoparticles are large, and when they are added to the soil, they are easy to aggregate into agglomerates, and the filling effect is not achieved. Therefore, in the present invention, the native enzyme and nanoparticles are set to synergistically solidify the soil. Both can not only play their own solidification effects, but the native enzyme can also modify the nanoparticles to improve the dispersibility of the nanoparticles, that is, the surfactant in the native enzyme can be adsorbed on the surface of the nanoparticles, improve the hydrophobicity of the nanoparticles, make it more evenly distributed in the soil, and improve the filling effect. Finally, since both the native enzyme and the nanoparticles can promote the polymerization reaction in the soil, after the native enzyme modifies the nanoparticles, the uniformly distributed nanoparticles can more fully play their "seed nucleation" effect, accelerate the polymerization reaction, and the increase in the gelled product makes the overall strength of the soil higher.

[0085] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Soil solidification material based on native enzyme modified nanoparticles and solid waste, characterized by: The soil solidification material comprises: Industrial solid waste, stimulants, native enzymes and nanomaterials.

2. The soil solidification material based on native enzyme-modified nanoparticles and solid waste according to claim 1, characterized in that: The weight components of the soil solidification material are: 8-12 parts of industrial solid waste, 2-6 parts of activator, 0-7 parts of native enzyme, and 0-2 parts of nano material.

3. The soil solidification material based on native enzyme-modified nanoparticles and solid waste according to claim 1, characterized in that: The industrial solid waste is selected from fly ash, slag, silicon powder, steel slag, carbide slag, quicklime or a mixture of two or more thereof.

4. The soil solidification material based on native enzyme modified nanoparticles and solid waste according to claim 1, characterized in that: The activator is selected from one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate or a mixture of two or more thereof.

5. The soil solidification material based on native enzyme modified nanoparticles and solid waste according to claim 1, characterized in that: The native enzyme is prepared from gramineous plants and soil insects through a protease extraction process.

6. The soil solidification material based on native enzyme-modified nanoparticles and solid waste according to claim 5, characterized in that: The extraction process of the native enzyme comprises the following steps: (1) Preparing crude enzyme solution of native enzyme: washing grass plants such as barley and insects such as ants obtained from nature, grinding and crushing plants in a mortar with a pestle, crushing animals with a meat grinder, collecting the crushed and filtered liquid of plants and animals, homogenizing with a homogenizer, mixing the slurry with a buffer solution at a ratio of 1:6, and extracting at a pH of 4 to 6 and a temperature of 25 to 35°C for 2 to 5 hours, and obtaining crude enzyme solution of native enzyme after centrifugation; (2) Salting out: Add the crude enzyme solution to a 60-80% ammonium sulfate solution, let stand at 4°C for 48-72 hours, centrifuge, take the supernatant, then add buffer, and dialyze for 12-24 hours. Perform salting out for at least 2-4 times; (3) Ion exchange chromatography: The enzyme solution after salting out is loaded onto a DEAE ion exchange column, the pH of the buffer is controlled to 7, the flow rate is 1-3 mL / min, and then eluted with 0.4-0.6 mol / L NaCl in Tris-HCl. After elution, the native enzyme solution purified by ion exchange chromatography can be obtained.

7. The soil solidification material based on native enzyme-modified nanoparticles and solid waste according to claim 1, characterized in that: The nano material is selected from one of nano SiO2, nano Al2O3, nano CaCO3 or a mixture of two or more thereof.

Citation Information

Cited By

  • Soil solidification complexing agent containing biological enzyme as well as preparation method and application of soil solidification complexing agent