Empty ladle weight control method
By controlling the stop blowing temperature of the converter and adding an appropriate amount of Taiwanese aluminum, lime and slag remover, adjusting the calcium-aluminum ratio and the parameters of argon gas blown at the bottom of the ladle, the problem of slag sticking and weight gain in the ladle was solved, and stable control of the empty ladle weight was achieved. , improving ladle turnover efficiency and reducing safety risks.
Patent Information
- Application Number
- CN202410783564.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
The increase in the weight of slag adhering to the ladle will lead to an increase in the weight of the empty ladle, affecting the quality of molten steel and the turnover efficiency of the ladle, posing safety risks.
By controlling the stop blowing temperature of the converter, adding Taiwan aluminum, lime and slag remover during the steel tapping process, adjusting the calcium-aluminum ratio, controlling the flow and back pressure of argon gas blown at the bottom of the ladle, arranging the LF refining station in a timely manner, and adjusting the production plan to reduce Sticky cold steel gains weight.
It effectively avoids ladle slag sticking, reduces ladle repair time and safety risks, maintains the stability of ladle weight, and improves ladle turnover efficiency.
Smart Images

Figure BDA0004897939680000061 
Figure BDA0004897939680000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel smelting, and more specifically discloses a method for controlling the weight of an empty ladle. Background Art
[0002] With the increase in the proportion of high-quality steel production, the ladle has become one of the important equipment for off-furnace refining, taking on more and more off-furnace refining tasks. However, the phenomenon of ladle slag sticking and weight increase has occurred more frequently in various steel mills, and this problem has troubled more and more steel mills. Ladle slag sticking mainly occurs on the ladle wall, ladle bottom and ladle mouth. If the ladle slag sticks seriously, it will cause many problems. When the ladle bottom sticks slag, it makes it difficult to clean the ladle air bricks during hot repair, which seriously affects the ladle bottom blowing effect and poses a serious threat to the quality of molten steel; slag and cold steel are formed at the ladle mouth, affecting the ladle slag turning; slag sticking to the ladle causes the weight of the ladle to increase, reducing the amount of molten steel after the furnace, affecting the purity and composition of the next batch of molten steel.
[0003] Research and analysis have shown that, whether it is a brick-built ladle or an integrally cast ladle, the thin layer of slag attached to the ladle lining surface is not the reaction product of slag and refractory materials, but the crystallization product after the ladle slag is condensed. Due to the formation of high melting point phases such as RO phase, SP and MA, and some of them grow into self-shaped spinel with RO phase as the core, the adhered slag layer is dense and firm. The main reason for slag sticking is that the calcium-aluminum ratio in the ladle slag is low, the adhered slag has a high melting point and high viscosity, and the slag melting point is mainly distributed between 1530 and 1750℃. High melting point substances such as CA2 (CaO·2Al2O3, 1780℃), CA6 (CaO·6Al2O3, 1880℃), C2AS (2CaO·Al2O3·SiO2, 1590℃) and MA (MgO·Al2O3, 2130℃) are formed in the slag. During the turnover of the ladle, the temperature of the slag layer decreases, and the thick and hard slag shell is tightly bonded to the ladle slag line bricks. The slag ring at the ladle mouth causes the ladle to be unable to be turned over or turned over completely when the casting slag is turned over. The remaining casting slag remains at the bottom of the ladle, affecting the increase in the weight of the ladle.
[0004] The capacity of Zhanjiang Steel's ladle is 350 tons, and the empty ladle weighs about 135-138 tons. During the use and turnover process, the ladle weight can reach 150 tons due to the weight gain caused by slag sticking. The steel types that cause the weight gain caused by slag sticking to the ladle are mainly low-carbon steel and medium-carbon (alloy) steel. Since the sticky slag is firmly bonded to the ladle lining, it is very difficult to remove the ladle during repair, which prolongs the repair time of the ladle, causes tight turnover of the ladle, and also causes overloading of the driving. This will pose a great safety hazard in the long run. In order to control the weight of the ladle and reduce the weight gain caused by slag sticking in the ladle, it is necessary to find a method for controlling the weight of the empty 350-ton ladle to reduce the sticky slag in the ladle and reduce the weight of the ladle. Summary of the invention
[0005] The present invention mainly provides a method for controlling the weight of an empty ladle, which can solve the problem that ladle slag is difficult to remove, resulting in an increase in the weight of the empty ladle and thus causing tight ladle turnover.
[0006] To solve the above technical problems, according to one aspect of the present invention, more specifically, a method for controlling the weight of an empty ladle comprises the following steps:
[0007] S1. Control the converter stop blowing temperature to avoid oxygen blowing and temperature rise of molten steel during the refining process, which will increase the alumina in the ladle slag and reduce the calcium-aluminum ratio;
[0008] S2. During the steel tapping process, ladle slag is modified by adding aluminum, lime and slag remover to control the calcium-aluminum ratio in the ladle slag to between 0.8 and 1.0;
[0009] S3. For low carbon steel, add 300-400kg of Taiwan aluminum and 800kg of lime into the ladle. When the empty ladle weight of the heat is ≥143 tons, the amount of lime added is adjusted to 1000kg.
[0010] S4. When the low carbon steel refining process path is non-LF, according to the empty ladle weight, add slag remover into the ladle as required during the steel tapping process;
[0011] S5. For medium carbon (alloy) steel grades, the amount of aluminum added during the steel-making process is added according to the converter stop blowing temperature. When the refining path does not contain LF, 800 kg of lime is added during the steel-making process; when the refining path contains LF, 1500 kg of lime is added during the steel-making process;
[0012] S6. Control the flow rate and back pressure of argon gas at the bottom of the ladle to avoid splashing during the refining process, which may cause the ladle to stick to the cold steel and increase its weight;
[0013] S7. Control the time from the end of ladle pouring to the end of slag turning. The time from the end of ladle pouring to the end of slag turning for the first batch of small / medium / major repair ladles on line is controlled to be ≤10min, and the time from the end of ladle pouring to the end of slag turning for other batches is controlled to be ≤15min, so as to reduce the sticking of cold steel to the bottom of the ladle and the weight gain of slag;
[0014] S8. Control the time interval between the small / medium / major repair ladles being put online. The time interval between the flameout of the new ladles to be put online after being baked to 1000℃ and the steel connection time is required to be ≤60min;
[0015] S9. For ladles with empty weight ≥145 tons, the ladles will be arranged to the LF refining station for production and processing through coordinating production plans. The temperature of the molten steel in the ladle will be uniformed through electrode heating to reduce the amount of cold steel sticking to the ladle wall and bottom.
[0016] Furthermore, in S1, the stop blowing temperature of low carbon steel is controlled to be ≥1630°C, and the stop blowing temperature of medium carbon (alloy) steel is controlled to be ≥1660°C.
[0017] Furthermore, in the S2, the main component of the slag remover is CaF2.
[0018] Furthermore, in S4, a slag remover is added into the ladle as required during the steel tapping process, and the specific rules are as follows:
[0019] (1) When the empty bag weight is less than 140 tons, the amount of slag remover added is 0;
[0020] (2) 140 tons ≤ empty bag weight < 142 tons: add 200 kg of slag remover;
[0021] (3) 142 tons ≤ empty bag weight < 146 tons: add 300 kg of slag remover;
[0022] (4) 146 tons ≤ empty bag weight < 155 tons: add 400 kg of slag remover.
[0023] Furthermore, in S5, the amount of aluminum added during the steel-making process is added according to the stop-blowing temperature of the converter, specifically: 200 kg of aluminum is added when the stop-blowing temperature is <1660°C, 300 kg of aluminum is added when 1660°C ≤ stop-blowing temperature ≤1670°C, and 400 kg of aluminum is added when the stop-blowing temperature is >1670°C.
[0024] Furthermore, in S6, the ladle bottom blowing pressure control range is 1.0-1.7Mpa, and the flow control range is 20-80Nm 3 / h.
[0025] The beneficial effect of the empty ladle weight control method of the present invention is that it can avoid the situation that the ladle is adhered to slag, which leads to the increase of the empty ladle weight. It can also avoid the situation that the slag is adhered to the ladle wall, which makes it very difficult to remove the ladle during repair, prolongs the ladle repair time, causes tight ladle turnover, and also causes overloading of the driving. If this happens for a long time, there will be a great safety hazard. DETAILED DESCRIPTION
[0026] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.
[0027] A method for controlling the weight of an empty ladle comprises the following steps:
[0028] The first step is to control the converter stop blowing temperature to avoid oxygen blowing and temperature rise of molten steel during the refining process, which will increase the alumina in the ladle slag and reduce the calcium-aluminum ratio. The stop blowing temperature of low carbon steel is controlled at ≥1630℃, and the stop blowing temperature of medium carbon (alloy) steel is controlled at ≥1660℃.
[0029] The second step is to modify the ladle slag during the steel-making process by adding aluminum, lime and slag remover (the main component is CaF2) to control the calcium-aluminum ratio in the ladle slag between 0.8-1.0.
[0030] The third step is to add 300-400kg of Taiwan aluminum and 800kg of lime into the ladle for low carbon steel. When the empty ladle weight of the furnace is ≥143 tons, the amount of lime added is adjusted to 1000kg.
[0031] Step 4: When the low carbon steel refining process path is non-LF, add slag remover into the ladle as required during the steel tapping process according to the empty ladle weight. The specific rules are as follows:
[0032] (1) When the empty bag weight is less than 140 tons, the amount of slag remover added is 0;
[0033] (2) 140 tons ≤ empty bag weight < 142 tons: add 200 kg of slag remover;
[0034] (3) 142 tons ≤ empty bag weight < 146 tons: add 300 kg of slag remover;
[0035] (4) 146 tons ≤ empty bag weight < 155 tons: add 400 kg of slag remover.
[0036] Step 5. For medium carbon (alloy) steel grades, the amount of alumina added during the steel-making process is based on the converter stop blowing temperature. Specifically, add 200kg of alumina when the stop blowing temperature is <1660℃, add 300kg of alumina when 1660℃≤stop blowing temperature≤1670℃, add 400kg of alumina when the stop blowing temperature is >1670℃. When the refining path does not contain LF, add 800kg of lime during the steel-making process; when the refining path contains LF, add 1500kg of lime during the steel-making process.
[0037] Step 6: Control the flow rate and back pressure of argon gas at the bottom of the ladle to avoid splashing during the refining process, which may cause the ladle to stick to the cold steel and increase its weight. The pressure control range of the ladle bottom blowing is 1.0-1.7Mpa, and the flow control range is 20-80Nm 3 / h.
[0038] Step 7. Control the time from the end of ladle pouring to the end of slag turning. The time from the end of ladle pouring to the end of slag turning for small / medium / major overhaul ladles is controlled to be ≤10min, and the time from the end of ladle pouring to the end of slag turning for other furnaces is controlled to be ≤15min, so as to reduce the sticking of cold steel to the bottom of the ladle and the weight gain of slag.
[0039] Step 8. Control the time interval for the small / medium / major repair ladles to be put online. The time interval from the flameout moment to the steel connection moment after the new ladles are baked to 1000℃ is required to be ≤60min.
[0040] Step 9. For ladles with empty weight ≥ 145 tons, arrange the ladles to the LF refining station for production and processing through coordinating production plans. By heating the ladle with electrodes, the temperature of the molten steel in the ladle is made uniform, reducing the amount of cold steel sticking to the ladle wall and bottom.
[0041] Embodiment 1
[0042] The above method is used to control the ladle weight on low carbon steel grades, and the relevant furnace parameters are shown in Table 1. The average ladle weight is 138.4 tons, the average weight gain is 240 kg, and the average calcium-aluminum ratio is 0.93.
[0043] Table 1 Low carbon steel ladle weight control heat information
[0044]
[0045] Embodiment 2
[0046] The above method is used to control the ladle weight on medium carbon (alloy) steel grades, and the relevant furnace parameters are shown in Table 2. The average ladle weight is 137.9 tons, the average weight gain is -66kg, and the average calcium-aluminum ratio is 1.26.
[0047] Table 2 Carbon steel ladle weight control heat information
[0048]
[0049] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention also fall within the protection scope of the present invention.
Claims
1. A method for controlling the weight of an empty ladle, characterized in that: The following steps are involved: S1. Control the converter stop blowing temperature to avoid oxygen blowing and temperature rise of molten steel during the refining process, which will increase the alumina in the ladle slag and reduce the calcium-aluminum ratio; S2. During the steel tapping process, ladle slag is modified by adding aluminum, lime and slag remover to control the calcium-aluminum ratio in the ladle slag to between 0.8 and 1.0; S3. For low carbon steel, add 300-400kg of Taiwan aluminum and 800kg of lime into the ladle. When the empty ladle weight of the heat is ≥143 tons, the amount of lime added is adjusted to 1000kg. S4. When the low carbon steel refining process path is non-LF, according to the empty ladle weight, add slag remover into the ladle as required during the steel tapping process; S5. For medium carbon (alloy) steel grades, the amount of aluminum added during the steel-making process is added according to the converter stop blowing temperature. When the refining path does not contain LF, 800 kg of lime is added during the steel-making process; when the refining path contains LF, 1500 kg of lime is added during the steel-making process; S6. Control the flow rate and back pressure of argon gas at the bottom of the ladle to avoid splashing during the refining process, which may cause the ladle to stick to the cold steel and increase its weight; S7. Control the time from the end of ladle pouring to the end of slag turning. The time from the end of ladle pouring to the end of slag turning for the first batch of small / medium / major repair ladles on line is controlled to be ≤10min, and the time from the end of ladle pouring to the end of slag turning for other batches is controlled to be ≤15min, so as to reduce the sticking of cold steel to the bottom of the ladle and the weight gain of slag; S8. Control the time interval between the small / medium / major repair ladles being put online. The time interval between the flameout of the new ladles to be put online after being baked to 1000℃ and the steel connection time is required to be ≤60min; S9. For ladles with empty weight ≥145 tons, the ladles will be arranged to the LF refining station for production and processing through coordinating production plans. The temperature of the molten steel in the ladle will be uniformed through electrode heating to reduce the amount of cold steel sticking to the ladle wall and bottom.
2. The method for controlling the empty ladle weight according to claim 1, characterized in that: In S1, the stop blowing temperature of low carbon steel is controlled to be ≥1630°C, and the stop blowing temperature of medium carbon (alloy) steel is controlled to be ≥1660°C.
3. The method for controlling the empty ladle weight according to claim 1, characterized in that: In the S2, the main component of the slag remover is CaF2.
4. The method for controlling the empty ladle weight according to claim 1, characterized in that: In S4, a slag remover is added into the ladle as required during the steel tapping process, and the specific rules are as follows: (1) When the empty bag weight is less than 140 tons, the amount of slag remover added is 0; (2) 140 tons ≤ empty bag weight < 142 tons: add 200 kg of slag remover; (3) 142 tons ≤ empty bag weight < 146 tons: add 300 kg of slag remover; (4) 146 tons ≤ empty bag weight < 155 tons: add 400 kg of slag remover.
5. The method for controlling the empty ladle weight according to claim 1, characterized in that: In S5, the amount of aluminum added during the steel-making process is added according to the stop-blowing temperature of the converter, specifically: 200 kg of aluminum is added when the stop-blowing temperature is less than 1660°C, 300 kg of aluminum is added when 1660°C≤stop-blowing temperature≤1670°C, and 400 kg of aluminum is added when the stop-blowing temperature is greater than 1670°C.
6. The method for controlling the empty ladle weight according to claim 1, characterized in that: In S6, the ladle bottom blowing pressure control range is 1.0-1.7Mpa, and the flow control range is 20-80Nm 3 / h.