High-strength TC10G titanium alloy wire for fastener and preparation and application of high-strength TC10G titanium alloy wire

By adding V, Fe and Sn elements to TC4 titanium alloy, and using solid solution aging treatment, TC10G titanium alloy wire was prepared, which solved the problem of insufficient strength and stability of TC4 titanium alloy in high temperature environment, and achieved more than 1350MPa Excellent tensile strength and excellent plasticity, suitable for high-strength fasteners.

CN118755997APending Publication Date: 2024-10-11INST OF METAL RESEARCH - CHINESE ACAD OF SCI +4
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410789694.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing TC4 titanium alloy has deficiencies in strength and hardenability, making it difficult to meet the stability and high strength requirements in high temperature environments, especially in fastener applications above 1350MPa.

Method used

By increasing the content of β-phase stabilizing element V on the basis of TC4 titanium alloy, adding trace amounts of Fe and Cu elements, and adding the neutral element Sn, and using solid solution aging treatment method, TC10G titanium alloy wire was prepared. Chemistry The ingredients are Al: 5.0% ~ 6.0%, V: 5. 0% ~ 6.0%, Sn: 1.50% ~ 2.50%, Fe: 0.35% ~ 1.0%, Cu: 0.35% ~ 1.0%, O ≤ 0.20%, and through electrode batching, vacuum consumable arc furnace smelting, forging, High-strength titanium alloy wire is obtained through processes such as rolling and drawing.

Benefits of technology

The solid solution aging strength of TC10G titanium alloy wire has been achieved to exceed 1350MPa. The microstructure has high stability and is suitable for high-strength fasteners. It has excellent plasticity and tensile strength and meets the requirements for use in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755997A_ABST
    Figure CN118755997A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength TC10G titanium alloy wire for a fastener as well as preparation and application of the high-strength TC10G titanium alloy wire. The alloy comprises chemical components in percentage by weight as follows: 5.0%-6.0% of Al, 5.0%-6.0% of V, 1.50%-2.50% of Sn, 0.35%-1.0% of Fe, 0.35%-1.0% of Cu and less than or equal to 0.20% of O, a matrix is Ti and inevitable impurity elements, and the total amount of the impurity elements is less than or equal to 0.30%. The diameter is 2.0-10.0 mm, and the alloy can be strengthened through solid solution aging treatment. After the alloy wire material is subjected to solid solution aging strengthening, a metallographic microstructure is a uniform alpha + beta transformation structure, the tensile strength is 1350 MPa or above, meanwhile, the alloy wire material has excellent plasticity, the ductility is kept to be 8% or above, the percentage reduction of area is kept to be 20% or above, and the alloy wire material can be well suitable for aviation high-strength single-face connection titanium alloy fasteners.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of high-strength titanium alloys, in particular to a wire material for titanium alloy fasteners with a strength of 1350 MPa or above, the alloy grade being defined as TC10G. The present invention also provides a method for preparing the alloy wire material. Background Art

[0002] Titanium alloy is an important structural material for manufacturing fasteners. Due to its high specific strength, titanium alloy fasteners have a significant weight reduction effect on aircraft and spacecraft. In addition, it has excellent corrosion resistance. In modern advanced aircraft manufacturing, its usage is increasing. The number of titanium alloy fasteners in a single machine is as high as hundreds of thousands to millions. It has become the most important "aerospace fastener" variety today. The amount of titanium alloy used has become one of the symbols to measure the level of a country's manufacturing technology.

[0003] TC4 titanium alloy (Ti-6Al-4V) is an α+β type duplex titanium alloy. This type of titanium alloy can be strengthened by heat treatment and is used in the manufacture of medium-strength (1200MPa level) fasteners. It is currently the most widely used and most stable titanium alloy at home and abroad. Considering the development of technology and the need to expand application fields, expanding the strength of this type of alloy has become an important development trend.

[0004] Alloying is a key means to improve material strength. The TC10G titanium alloy of the present invention increases the content of β-phase stabilizing element V on the basis of TC4 alloy, and also adds trace amounts of Fe and Cu elements, which make up for the problems of insufficient strength and unsatisfactory hardenability of TC4 alloy. The neutral element Sn is added to the alloy to ensure its stability in high-temperature environments. Currently, it can be used in high-temperature environments of 400°C.

[0005] As a high-strength dual-phase titanium alloy, TC10G has the advantages of significant heat treatment strengthening effect, excellent mechanical properties, good hardenability, and stable microstructure. After solution aging treatment, the tensile strength can exceed 1350MPa without significantly reducing the plasticity. It is an excellent high-strength titanium alloy structural material, especially suitable for high-strength titanium alloy fasteners. Summary of the invention

[0006] The purpose of the present invention is to provide a high-strength TC10G titanium alloy wire for fasteners and a preparation method thereof. The alloy wire has a solid solution aging strength of more than 1350MPa, has good plasticity, and has high microstructural stability and a uniform and fine dual-phase structure, which meets the service conditions of high-strength titanium alloy fasteners.

[0007] In order to achieve the above object, the technical solution provided by the present invention is as follows:

[0008] A high-strength TC10G titanium alloy wire for fasteners, characterized in that the mass percentages of the alloy chemical components are: Al: 5.0%-6.0%, V: 5.0%-6.0%, Sn: 1.50%-2.50%, Fe: 0.35%-1.0%, Cu: 0.35%-1.0%, O≤0.20%, the matrix is ​​Ti and unavoidable impurity elements, and the total amount of impurity elements is ≤0.30%.

[0009] The high-strength TC10G titanium alloy wire has a β transformation temperature of ≥930°C, and the preferred chemical composition mass percentages are: Al: 5.3% to 5.7%, V: 5.3% to 5.7%, Sn: 1.70% to 2.30%, Fe: 0.45% to 0.65%, Cu: 0.45% to 0.65%, and O: 0.13% to 0.18%.

[0010] The present invention discloses a method for preparing TC10G wire, which is as follows:

[0011] (1) Electrode: The ingredients are prepared according to the following mass percentages: Al: 5.0% to 6.0%, V: 5.0% to 6.0%, Sn: 1.50% to 2.50%, Fe: 0.35% to 1.0%, Cu: 0.35% to 1.0%, O≤0.20%, the matrix is ​​Ti and unavoidable impurity elements, and the total amount of impurity elements is ≤0.40%; AlV binary alloy, Ti80Sn binary alloy, aluminum beans, Fe powder, Cu powder, TiO2 powder, and sponge titanium are mixed and pressed into electrode blocks, and the electrodes are welded.

[0012] (2) Melting: Melting in a vacuum consumable arc furnace for ≥ 2 times (preferably 3 times) to obtain a TC10G titanium alloy ingot;

[0013] (3) Forging: The TC10G titanium alloy ingot is forged into a bar at 1100-1200°C (preferably 1130-1170°C); the bar forging is performed at 1000-1050°C (preferably 1020-1030°C); the fine forging is performed at 960-1000°C (preferably 970-980°C) to obtain a TC10G titanium alloy bar blank;

[0014] (4) Rolling: The TC10G titanium alloy bar billet is continuously rolled at 860-900° C. (preferably 870-880° C.) to obtain a TC10G titanium alloy wire billet;

[0015] (5) Wire drawing and finished product heat treatment: TC10G titanium alloy wire billet is drawn at 600-750°C (preferably 680-720°C), the wire drawing deformation is 20%-80% (preferably 30%-50%), the finished product heat treatment system is 680-780°C (preferably 700-740°C), kept warm for 1.5-3.5 hours (preferably 2-3 hours), and air-cooled to obtain TC10G titanium alloy annealed wire.

[0016] The present invention relates to a wire material for titanium alloy fasteners with a grade of 1350MPa or above, wherein the alloy grade is defined as TC10G. After being solid solution-aged and strengthened, the metallographic microstructure of the alloy wire material is a uniform α+β transformation structure, and the alloy wire material can be well applied to aviation high-strength single-sided connection titanium alloy fasteners.

[0017] The high-strength TC10G titanium alloy wire has a wire diameter of 2.0 mm to 10.0 mm. After solution aging treatment, the alloy wire is suitable for the manufacture of 1350 MPa-grade fasteners. The solution aging system is: 900°C (±15°C), keep warm for 60min±5min and then quench in running water at room temperature; 540°C (±10°C), keep warm for 4h±0.25h and then air cool. The metallographic microstructure is a uniform α+β transformation structure, and the transverse microstructure is specifically a structure processed in the α-β two-phase region. The original grain boundary β is broken and there is no continuous grain boundary α. The alloy has a tensile strength of more than 1350 MPa and excellent plasticity, with the elongation maintained at more than 8% and the cross-sectional shrinkage maintained at more than 20%.

[0018] The present invention has the following advantages and beneficial effects:

[0019] (1) The TC10G high-strength titanium alloy of the present invention is a high-strength dual-phase titanium alloy with a stable structure obtained by alloying the TC4 titanium alloy by adjusting the content of the β-stabilizing element V, increasing the content of the β-stabilizing elements Cu and Fe, controlling the content of the α-stabilizing element O, and increasing the neutral element Sn.

[0020] (2) The TC10G high-strength titanium alloy of the present invention adopts small-particle sponge titanium, ≤1mmAlV binary alloy, analytically pure Fe, Cu, TiO2, aluminum beans and low-melting-point TiSn binary alloy, mixed materials and pressed electrodes, and smelted in a vacuum consumable arc furnace three times to obtain an ingot with low impurity elements and high composition uniformity.

[0021] (3) The TC10G high-strength titanium alloy wire of the present invention has a strength of more than 1350 MPa after solid solution aging strengthening, has a good matching degree between strength and plasticity, and has a stable and uniform metallographic structure, which is suitable for the service requirements of high-strength titanium alloy fasteners. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the transverse microstructure of the solution-aged wire with a diameter of 6.64 mm in Example 1 (500 times)

[0023] Figure 2 This is the transverse microstructure of the solution-aged wire with a diameter of 3.01 mm in Example 2 (500 times)

[0024] Figure 3 This is the transverse microstructure of the solution-aged wire with a diameter of 2.98 mm in Example 3 (500 times)

[0025] Figure 4 This is the transverse microstructure of the solution-aged wire with a diameter of 8.47 mm in Example 4 (500 times)

[0026] Depend on Figure 1-4 It can be seen that the solid solution aging microstructure of the TC10G titanium alloy wire of the invention is a uniform α+β transformation structure, the white is the α phase structure, the black is the β transformation structure, and the transverse microstructure is specifically the structure processed in the α-β two-phase region. The original grain boundary β is broken and there is no continuous grain boundary α. This microstructure can well meet the use requirements of fasteners. DETAILED DESCRIPTION

[0027] The preparation process of the high-strength TC10G titanium alloy wire for fasteners in the following embodiments and comparative examples is as follows:

[0028] A high-strength TC10G titanium alloy wire for fasteners is prepared by mixing AlV binary alloy with a particle size of ≤1mm, Ti80Sn binary alloy, analytically pure aluminum beans, analytically pure Fe powder, analytically pure Cu powder, analytically pure TiO2 powder, and sponge titanium with a particle size of 3-12.7mm, and then pressing them into electrode blocks, welding electrodes, and melting them three times in a vacuum consumable arc furnace into cylindrical ingots (diameter 600mm); the ingots are forged at 1150℃ (±50℃) into square bars (cross-section side length 300mm), and the bars are forged at 1025℃ (±25℃) The process is as follows: the first step is to forge a cylindrical rod blank with a diameter of 140 mm, and the final forging is performed at 980° C. (±20° C.) to obtain a cylindrical rod blank with a diameter of 100 mm; the rod blank is continuously rolled at 880° C. (±20° C.) with continuous temperature and speed control, and the final rolling temperature is between 750 and 850° C. to obtain a wire blank (with a diameter of 8 mm to 16 mm); the wire blank is drawn at ≤750° C., and the total deformation of the wire drawing is 20 to 80%; the finished product is heat treated at a temperature of 680 to 780° C., kept warm for 2 hours, and air-cooled to obtain a TC10G titanium alloy annealed wire (with a diameter of 2 mm to 10 mm).

[0029] Embodiment 1:

[0030] The alloy composition is Ti-5.48Al-5.48V-2.27Sn-0.43Fe-0.44Cu-0.15O (the number before each element represents its mass percentage in the alloy, the balance is Ti, and the total mass of impurity elements (including Si, Ni, B, Y, etc., the same below) in the alloy is ≤0.30%), the final rolling temperature is between 840°C, the diameter of the wire billet after rolling is 11.2mm, the wire billet is drawn at 700°C, the drawing deformation is 56.3%, the finished product heat treatment temperature is 720°C, the temperature is kept for 2 hours, and air-cooled to prepare a finished annealed wire with a diameter of 6.64mm. The β transformation temperature measured by metallographic method (test standard: GB / T 23605 titanium alloy β transformation temperature determination method) is 945°C±5°C.

[0031] After the wire with a diameter of 6.64 mm was treated with 900℃ / 1h / WQ (water quenching) + 540℃ / 4h / AC (air cooling), the metallographic microstructure was Figure 1 As shown, it is a uniform α+β transformation structure, specifically a structure processed in the α-β two-phase region, the original grain boundary β is broken, and there is no continuous grain boundary α. The mechanical properties of the solution aging state (test standard: GB / T 228.1 Metal material tensile test Part 1: Room temperature test method) are shown in Table 1. The tensile strength Rm is above 1350MPa, the elongation A is above 8%, and the cross-sectional shrinkage Z is above 20%, which has excellent strength and plasticity.

[0032] Table 1 Solution-aging mechanical properties of wire with a diameter of 6.64 mm

[0033]

[0034] Embodiment 2:

[0035] The alloy composition is Ti-5.48Al-5.48V-2.27Sn-0.43Fe-0.44Cu-0.15O (the number before each element represents its mass percentage in the alloy, the remainder is Ti, and the total mass of impurity elements in the alloy is ≤0.30%), the final rolling temperature is between 828°C, the diameter of the wire billet after rolling is 8.0mm, the wire billet is drawn at 710°C, the drawing deformation is 77.4%, the finished product heat treatment temperature is 740°C, kept warm for 2 hours, air cooled, and prepared into a finished annealed wire with a diameter of 3.01mm. The β transformation temperature measured by metallographic method (test standard: GB / T23605 titanium alloy β transformation temperature determination method) is 945°C±5°C.

[0036] After the wire with a diameter of 3.01 mm was treated at 890℃ / 1h / WQ (water quenching) + 540℃ / 4h / AC (air cooling), the metallographic microstructure is shown. Figure 2As shown in Table 2, it is a uniform α+β transformation structure, specifically a structure processed in the α-β two-phase region, with the original grain boundary β broken and no continuous grain boundary α. The mechanical properties of the solution aging state (test standard: GB / T 228.1 Metallic material tensile test Part 1: Room temperature test method) are shown in Table 2. The tensile strength Rm is above 1350MPa, the elongation A is above 8%, and the cross-sectional shrinkage Z is above 20%, which has excellent strength and plasticity.

[0037] Table 2 Solution aging mechanical properties of wire with a diameter of 3.01 mm

[0038]

[0039]

[0040] Embodiment 3:

[0041] The alloy composition is Ti-5.80Al-5.85V-2.27Sn-0.50Fe-0.45Cu-0.18O (the number before each element represents its mass percentage in the alloy, the remainder is Ti, and the total mass of impurity elements in the alloy is ≤0.30%), the final rolling temperature is between 816°C, the diameter of the wire billet after rolling is 7.8mm, the wire billet is drawn at 700°C, the drawing deformation is 76.2%, the finished product heat treatment temperature is 740°C, the temperature is kept for 2 hours, and air-cooled to prepare a finished annealed wire with a diameter of 2.98mm. The β transformation temperature measured by metallographic method (test standard: GB / T23605 titanium alloy β transformation temperature determination method) is 940°C±5°C.

[0042] After the wire with a diameter of 2.98 mm was treated with 885℃ / 1h / WQ (water quenching) + 540℃ / 4h / AC (air cooling), the metallographic microstructure is shown. Figure 3 As shown in Table 3, it is a uniform α+β transformation structure, specifically a structure processed in the α-β two-phase region, with the original grain boundary β broken and no continuous grain boundary α. The mechanical properties of the solution aging state (test standard: GB / T 228.1 Metal material tensile test Part 1: Room temperature test method) are shown in Table 3. The tensile strength Rm is above 1350MPa, the elongation A is above 8%, and the cross-sectional shrinkage Z is above 20%, which has excellent strength and plasticity.

[0043] Table 3 Solution aging mechanical properties of wire with a diameter of 2.98 mm

[0044]

[0045] Embodiment 4:

[0046] The alloy composition is Ti-5.80Al-5.85V-2.27Sn-0.50Fe-0.45Cu-0.18O (the number before each element represents its mass percentage in the alloy, the remainder is Ti, and the total mass of impurity elements in the alloy is ≤0.30%), the final rolling temperature is between 845°C, the diameter of the wire billet after rolling is 11.2mm, the wire billet is drawn at 700°C, the drawing deformation is 32.5%, the finished product heat treatment temperature is 720°C, the temperature is kept for 2 hours, and air-cooled to prepare a finished annealed wire with a diameter of 8.47mm. The β transformation temperature measured by metallographic method (test standard: GB / T23605 titanium alloy β transformation temperature determination method) is 940°C±5°C.

[0047] After the wire with a diameter of 8.47 mm was treated with 895℃ / 1h / WQ (water quenching) + 540℃ / 4h / AC (air cooling), the metallographic microstructure was Figure 4 As shown in Table 4, it is a uniform α+β transformation structure, specifically a structure processed in the α-β two-phase region, with the original grain boundary β broken and no continuous grain boundary α. The mechanical properties of the solution aging state (test standard: GB / T 228.1 Metallic material tensile test Part 1: Room temperature test method) are shown in Table 4. The tensile strength Rm is above 1350MPa, the elongation A is above 8%, and the cross-sectional shrinkage Z is above 20%, which has excellent strength and plasticity.

[0048] Table 4 Solution aging mechanical properties of wire with a diameter of 8.47 mm

[0049]

[0050] Comparative Example 1:

[0051] Alloy composition Ti-6.28Al-5.84V-2.12Sn-0.63Fe-0.58Cu-0.15O (the number before each element represents its mass percentage in the alloy, the remainder is Ti, and the total mass of impurity elements in the alloy is ≤0.30%). The alloy composition Al of Comparative Example 1 is higher than the mass percentage upper limit of the claim (6%), the final rolling temperature is between 824°C, and the wire billet is rolled into a wire billet with a diameter of 11.2 mm, which exceeds the specified finished wire diameter of 10 mm, and the wire drawing is not performed according to the above process or the wire drawing deformation of 20 to 80% of the claim. The finished wire billet is directly heat treated at a heat treatment temperature of 704°C, kept warm for 2 hours, and air-cooled to prepare a finished annealed wire with a diameter of 11 mm. After 900°C / 1h / WQ (water quenching) + 540°C / 4h / AC (air cooling) treatment, the alloy mechanical properties (test standard: GB / T 228.1 Tensile test of metallic materials Part 1: Room temperature test method) As shown in Table 5, it can be seen that the tensile strength Rm exceeds 1350MPa, but the elongation A is less than 8%, the plasticity is significantly reduced, and the comprehensive performance is poor, which does not meet the use requirements of high-strength TC10G titanium alloy fasteners.

[0052] Table 5 Solution aging mechanical properties of 11 mm diameter wire (high Al undrawn)

[0053]

[0054]

[0055] Comparative Example 2:

[0056] Alloy composition Ti-5.68Al-6.05V-2.02Sn-0.64Fe-0.60Cu-0.14O (the number before each element represents its mass percentage in the alloy, the remainder is Ti, and the total mass of impurity elements in the alloy is ≤0.30%), the alloy composition V of the comparative example 2 is higher than the mass percentage upper line of the claim (6%), the final rolling temperature is between 823°C, and the wire billet with a diameter of 11.2mm is rolled, which exceeds the specified finished wire diameter of 10mm, and the wire drawing is not performed according to the above process or the wire drawing deformation of 20-80% of the claim. The finished wire billet is directly heat treated at a heat treatment temperature of 704°C, kept warm for 2 hours, and air-cooled to prepare a finished annealed wire with a diameter of 11mm. After 900°C / 1h / WQ (water quenching) + 540°C / 4h / AC (air cooling) treatment, the alloy mechanical properties (test standard: GB / T 228.1 Tensile test of metallic materials Part 1: Room temperature test method) As shown in Table 6, it can be seen that the tensile strength Rm exceeds 1350MPa, but the elongation A is less than 8%, the cross-sectional shrinkage Z is less than 20%, the plasticity is significantly reduced, and the comprehensive performance is poor, which does not meet the use requirements of high-strength TC10G titanium alloy fasteners.

[0057] Table 6 Solution aging mechanical properties of 11 mm diameter wire (high V without wire drawing deformation)

[0058]

[0059] The above-described embodiments and comparative examples are merely typical examples of the present invention.

Claims

1. A high-strength TC10G titanium alloy wire for fasteners, characterized in that: The mass percentages of the chemical components of the alloy are: Al: 5.0% to 6.0% (preferably 5.3% to 5.7%), V: 5.0% to 6.0% (preferably 5.3% to 5.7%), Sn: 1.50% to 2.50% (preferably 1.70% to 2.30%), Fe: 0.35% to 1.0% (preferably 0.45% to 0.65%), Cu: 0.35% to 1.0% (preferably 0.45% to 0.65%), O≤0.20% (preferably 0.13% to 0.18%), and the matrix is ​​Ti and unavoidable impurity elements.

2. The TC10G titanium alloy wire according to claim 1, characterized in that: The total mass content of impurity elements is ≤0.40%, preferably the total mass content of impurity elements is ≤0.30%.

3. A method for preparing the high-strength TC10G titanium alloy wire for fasteners according to claim 1 or 2, characterized in that: The specific steps are as follows: (1) Electrode: Mix the materials according to the required element mass percentage, press them into electrode blocks after mixing, and weld the electrodes; (2) Melting: Melting in a vacuum consumable arc furnace for ≥2 times (preferably 3-4 times) to obtain a TC10G titanium alloy ingot; (3) Forging: The TC10G titanium alloy ingot is forged into a bar at 1100-1200°C (preferably 1130-1170°C); the bar forging is performed at 1000-1050°C (preferably 1020-1030°C); the fine forging is performed at 960-1000°C (preferably 970-980°C) to obtain a TC10G titanium alloy bar blank; (4) Rolling: The TC10G titanium alloy bar billet is continuously rolled at 860-900° C. (preferably 870-880° C.) to obtain a TC10G titanium alloy wire billet; (5) Wire drawing and finished product heat treatment: TC10G titanium alloy wire billet is drawn at 600-750°C (preferably 680-720°C), the wire drawing deformation is 20%-80% (preferably 30%-50%), the finished product heat treatment temperature is 680-780°C (preferably 700-740°C), the heat preservation is 1.5-3.5 hours (preferably 2-3 hours), and air cooling is performed to obtain TC10G titanium alloy annealed wire.

4. The method for preparing the TC10G titanium alloy wire according to claim 3, characterized in that: In the titanium alloy, Al and V are derived from AlV binary alloy and aluminum beans with a particle size of ≤1 mm, Sn is derived from Ti80Sn binary alloy, Fe and Cu are derived from pure element Fe powder and Cu powder respectively, O is mainly derived from sponge titanium and TiO2 powder, and the matrix Ti is derived from sponge titanium with a particle size of 3 to 12.7 mm. Step 1) AlV binary alloy, Ti80Sn binary alloy, aluminum beans, Fe powder, Cu powder, TiO2 powder, and sponge titanium are mixed and pressed into an electrode block, and the electrode is welded.

5. The method for preparing the TC10G titanium alloy wire according to any one of claims 3-4, characterized in that: The wire diameter is 2.0mm~10.0mm. After solution aging treatment, the alloy wire is suitable for the manufacture of 1350MPa grade fasteners. The solution aging system is: 900℃ (±15℃), keep warm for 60min±5min and then quench in running water at room temperature; 540℃ (±10℃), keep warm for 4h±0.25h and then air cool. The metallographic microstructure is a uniform α+β transformation structure with a tensile strength of more than 1350MPa. It also has excellent plasticity, with the elongation maintained at more than 8% and the cross-sectional shrinkage maintained at more than 20%.

6. Use of the high-strength TC10G titanium alloy wire for fasteners according to claim 1 or 2 or the TC10G titanium alloy wire prepared by the preparation method according to any one of claims 3 to 5 as a titanium alloy fastener.

7. The use of the TC10G titanium alloy wire according to claim 6, characterized in that: The titanium alloy fasteners are titanium alloy fasteners used on aircraft or spacecraft.

Citation Information

Cited By

  • Preparation method of TC10 titanium alloy large-disc round wire for fastener

    CN119553113A