High-strength and high-brightness electronic watch material and preparation method thereof

Through alloy materials of Co, Zn, Mg, Cu, Cr, La, Ti, Al and other metal elements and their preparation technology, the problem of insufficient strength and brightness of watch materials has been solved, and high-strength and high-brightness electronic watch materials have been realized, improving tensile strength and yield strength.

CN118756004APending Publication Date: 2024-10-11ANHUI XINBO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410813981.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing watch materials are difficult to meet the market's higher demand for high-end smart watches in terms of strength and brightness.

Method used

It adopts alloy materials of metal elements such as Co, Zn, Mg, Cu, Cr, La, Ti, Al, etc., and goes through the steps of melting, refining, casting, homogenization treatment, extrusion molding, solid solution treatment, aging treatment and surface treatment. Preparation of high-strength and bright electronic watch materials.

Benefits of technology

The high strength and high brightness of the watch material is achieved, and the uniformity and gloss of the material are improved through element synergy and processing technology, reducing cracking and improving the tensile strength and yield strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-strength and high-brightness electronic watch material and a preparation method thereof, and relates to the technical field of watch material manufacturing. The invention provides a high-strength and high-brightness electronic watch material which comprises the following chemical components in percentage by mass: 0.01-0.1% of Co, 0.01-0.2% of Zn, 0.05-0.5% of Mg, 0-0.1% of Cu, less than or equal to 0.01% of Cr, 0.01-0.2% of La, 0.01-0.5% of Ti and the balance of Al and inevitable impurities, and the total amount is 100%. The watch material prepared by the invention has relatively high tensile strength, yield strength and surface glossiness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of watch material manufacturing, and in particular to a high-strength and high-brightness electronic watch material and a preparation method thereof. Background Art

[0002] There are many raw materials for making watches, and there are strict requirements on the performance, surface state and dimensional accuracy of the materials. Stainless steel has always been a relatively high-end material for making watches. It is very strong and wear-resistant. In smart watches, it is mainly used as the middle frame and frame material, generally 316L. The molding and surface treatment processes include forging, powder metallurgy, coating, polishing, etching, sandblasting, brushing, etc. It is a material commonly used by mainstream watch manufacturers such as Apple and Huawei. Aluminum alloy, zinc alloy, zinc alloy and other alloy materials are widely used in watches because of the high design freedom of alloy materials. As the market has higher demands on the strength and brightness of watch materials, the development of a high-strength and high-brightness electronic watch material is of great significance to meet market demand. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a high-strength and high-brightness electronic watch material and a preparation method thereof.

[0004] The invention provides a high-strength and high-brightness electronic watch material, whose chemical composition, in terms of mass percentage, includes: Co: 0.01-0.1%, Zn: 0.01-0.2%, Mg: 0.05-0.5%, Cu: 0-0.1%, Cr≤0.01%, La: 0.01-0.2%, Ti: 0.01-0.5%, and the remainder is Al and unavoidable impurities, with a total amount of 100%.

[0005] Preferably, the total mass fraction of Cu, Cr and Ti is no more than 0.4%.

[0006] Preferably, the mass fraction of Ti is 0.01-0.3%.

[0007] The present invention also provides a method for preparing a high-strength and high-brightness electronic watch material, comprising the following steps:

[0008] S1. Add metal raw materials according to the chemical composition of the watch material and melt them to obtain a crude melt;

[0009] S2. Under a protective gas atmosphere, the crude melt is refined, allowed to stand and heat-insulated, and slag-removed to obtain a refined melt;

[0010] S3, casting the refined melt to obtain an ingot;

[0011] S4, homogenizing the ingot, extruding, solutionizing, and aging to obtain a profile;

[0012] S5. Performing surface treatment on the profile to obtain a watch material.

[0013] Preferably, in said S1, said melting comprises firstly keeping the temperature at 650-720°C for 0.5-1h, and then keeping the temperature at 720-800°C for 0.5-1h.

[0014] Preferably, in said S2, the protective gas is nitrogen.

[0015] Preferably, in S2, the refining temperature is 720-750°C and the holding time is 0.5-1h.

[0016] Preferably, in S3, the casting method includes a hot top method or an oil-gas sliding method.

[0017] Preferably, in said S4, the homogenization treatment comprises firstly keeping the temperature at 350-450°C for 3-6 hours, and then keeping the temperature at 500-580°C for 4-8 hours.

[0018] Preferably, in S4, the extrusion speed of the extrusion molding is 1-10 m / min.

[0019] Preferably, in said S4, the solution treatment comprises maintaining the temperature at 380-400° C. for 3-6 hours.

[0020] Preferably, in S4, the aging treatment comprises first heating to 150-170°C at 1-2°C / min and keeping warm for 3-6h, then heating to 170-190°C at 0.5-1°C / min and keeping warm for 4-8h, and cooling to below 40°C with strong wind.

[0021] Preferably, in S5, the surface treatment includes one or more of polishing, wire drawing, and anodizing.

[0022] The beneficial effects of the present invention are:

[0023] The high-strength and high-brightness electronic watch material proposed by the present invention includes metal elements such as Co, Zn, Mg, Cu, Cr, La, Ti, and Al. The elements work synergistically with each other, and the watch material prepared by the present invention has the characteristics of high strength and high brightness. The addition of Cu, Cr, and Ti can improve the glossiness of the watch material on the one hand, and the network structure of the alloy phase formed by Cu and Ti and the alloy phase formed by Cr and Ti can help improve the strength of the watch material on the other hand. Co and La are uniformly dispersed and precipitated during the homogenization process, and work synergistically with Cu and Mg to inhibit grain coarsening, which can effectively reduce the occurrence of cracking. The addition of Zn and Mg helps to improve the strength of the watch material. The present invention obtains a profile by homogenizing the ingot, extruding, solution treating, and aging, and the profile is surface treated to obtain the watch material, wherein the homogenization treatment and aging treatment adopt a two-stage treatment method, which helps to improve the uniformity of each element in the watch material and improve the strength of the watch material; the glossiness of the watch material is effectively improved after surface treatment. The watch material prepared by the present invention has the characteristics of high strength and high brightness. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is described in detail through specific embodiments.

[0025] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.

[0026] Example 1

[0027] A method for preparing a high-strength and high-brightness electronic watch material comprises the following steps:

[0028] S1. Add metal raw materials according to the chemical composition of the watch material (see Table 1 for details), and melt to obtain a crude melt; the melting includes first keeping the temperature at 650°C for 1 hour, and then keeping the temperature at 750°C for 0.5 hour;

[0029] S2. Under a nitrogen atmosphere, the crude melt is refined at 730° C., kept at this temperature for 0.5 h, and subjected to slag removal to obtain a refined melt;

[0030] S3, casting the molten metal by hot top method to obtain an ingot;

[0031] S4, subjecting the ingot to homogenization treatment, extrusion molding, solution treatment, and aging treatment to obtain a profile; the homogenization treatment includes first keeping at 420°C for 3 hours and then keeping at 550°C for 6 hours; the extrusion molding extrusion speed is 3m / min; the solution treatment includes keeping at 380°C for 3 hours; the aging treatment includes first heating to 160°C at 2°C / min and keeping for 4 hours, then heating to 180°C at 0.5°C / min and keeping for 5 hours, and cooling to below 40°C with strong wind;

[0032] S5. Performing surface treatment on the profile to obtain watch material; the surface treatment includes polishing and anodizing.

[0033] Example 2

[0034] A method for preparing a high-strength and high-brightness electronic watch material comprises the following steps:

[0035] S1. Adding metal raw materials according to the chemical composition of the watch material (see Table 1 for details), and melting to obtain a crude melt; the melting includes first keeping the temperature at 680°C for 1 hour, and then keeping the temperature at 780°C for 0.5 hour;

[0036] S2. Under a nitrogen atmosphere, the crude melt is refined at 730° C., kept at this temperature for 0.5 h, and subjected to slag removal to obtain a refined melt;

[0037] S3, casting the molten metal by hot top method to obtain an ingot;

[0038] S4, subjecting the ingot to homogenization treatment, extrusion molding, solution treatment, and aging treatment to obtain a profile; the homogenization treatment includes first keeping the temperature at 350°C for 3 hours and then keeping the temperature at 580°C for 6 hours; the extrusion molding extrusion speed is 2m / min; the solution treatment includes keeping the temperature at 380°C for 3 hours; the aging treatment includes first heating to 160°C at 2°C / min and keeping the temperature for 4 hours, then heating to 180°C at 1°C / min and keeping the temperature for 5 hours, and cooling to below 40°C with strong wind;

[0039] S5. Performing surface treatment on the profile to obtain watch material; the surface treatment includes polishing and anodizing.

[0040] Example 3

[0041] A method for preparing a high-strength and high-brightness electronic watch material comprises the following steps:

[0042] S1. Add metal raw materials according to the chemical composition of the watch material (see Table 1 for details), and melt to obtain a crude melt; the melting includes first keeping the temperature at 650°C for 1 hour, and then keeping the temperature at 750°C for 0.5 hour;

[0043] S2. Under a nitrogen atmosphere, the crude melt is refined at 750° C., kept at this temperature for 0.5 h, and subjected to slag removal to obtain a refined melt;

[0044] S3, casting the molten metal by hot top method to obtain an ingot;

[0045] S4, subjecting the ingot to homogenization treatment, extrusion molding, solution treatment, and aging treatment to obtain a profile; the homogenization treatment includes first keeping the temperature at 400°C for 3 hours and then keeping the temperature at 550°C for 6 hours; the extrusion molding extrusion speed is 2m / min; the solution treatment includes keeping the temperature at 380°C for 3 hours; the aging treatment includes first heating to 160°C at 1°C / min and keeping the temperature for 3 hours, then heating to 180°C at 0.5°C / min and keeping the temperature for 5 hours, and cooling to below 40°C with strong wind;

[0046] S5. Performing surface treatment on the profile to obtain watch material; the surface treatment includes polishing and anodizing.

[0047] Example 4

[0048] A method for preparing a high-strength and high-brightness electronic watch material comprises the following steps:

[0049] S1. Add metal raw materials according to the chemical composition of the watch material (see Table 1 for details), and melt to obtain a crude melt; the melting includes first keeping the temperature at 650°C for 1 hour, and then keeping the temperature at 750°C for 0.5 hour;

[0050] S2. Under a nitrogen atmosphere, the crude melt is refined at 730° C., kept at this temperature for 0.5 h, and subjected to slag removal to obtain a refined melt;

[0051] S3, casting the molten metal by hot top method to obtain an ingot;

[0052] S4, subjecting the ingot to homogenization treatment, extrusion molding, solution treatment, and aging treatment to obtain a profile; the homogenization treatment includes first keeping at 400°C for 3 hours and then keeping at 560°C for 6 hours; the extrusion molding extrusion speed is 3m / min; the solution treatment includes keeping at 400°C for 3 hours; the aging treatment includes first heating to 150°C at 2°C / min and keeping for 4 hours, then heating to 190°C at 0.5°C / min and keeping for 5 hours, and cooling to below 40°C with strong wind;

[0053] S5. Performing surface treatment on the profile to obtain watch material; the surface treatment includes polishing and anodizing.

[0054] The chemical compositions of the watch materials in Examples 1-4 of the present invention are shown in Table 1.

[0055] Table 1 Chemical composition of watch materials

[0056] alloy Co / % Zn / % Mg / % Cu / % Cr / % La / % Ti / % Al / % Example 1 0.03 0.12 0.37 0.03 0.01 0.18 0.19 margin Example 2 0.07 0.15 0.37 0.05 0.01 0.15 0.24 margin Example 3 0.06 0.08 0.31 0.03 0.01 0.12 0.25 margin Example 4 0.06 0.12 0.28 0.05 0.01 0.18 0.21 margin

[0057] The watch materials prepared in the above Examples 1-4 were tested for tensile strength, yield strength and glossiness. The test results are shown in Table 2.

[0058] Table 2 Performance test data of watch materials

[0059] project Tensile strength / Mpa Yield strength / Mpa Surface gloss / Gu Example 1 385 345 442 Example 2 398 360 480 Example 3 372 336 510 Example 4 386 358 467

[0060] It can be seen from the data in Table 2 that the watch material prepared by the present invention has high tensile strength, yield strength and surface gloss. In summary, the watch material provided by the present invention has the characteristics of high strength and high gloss.

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high-strength and high-brightness electronic watch material, characterized in that: Its chemical composition includes, by mass percentage: Co: 0.01-0.1%, Zn: 0.01-0.2%, Mg: 0.05-0.5%, Cu: 0-0.1%, Cr≤0.01%, La: 0.01-0.2%, Ti: 0.01-0.5%, the remainder is Al and unavoidable impurities, the total amount is 100%.

2. A high-strength and high-brightness electronic watch material according to claim 1, characterized in that: The total mass fraction of Cu, Cr and Ti is no more than 0.4%; the mass fraction of Ti is 0.01-0.3%.

3. A method for preparing the high-strength and high-brightness electronic watch material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Add metal raw materials according to the chemical composition of the watch material, and melt them to obtain a crude melt; S2. Refine the crude melt, let it stand and keep it warm, and remove slag to obtain a refined melt under a protective gas atmosphere; S3. Cast the refined melt to obtain an ingot; S4, homogenizing the ingot, extruding, solutionizing, and aging to obtain a profile; S5. Performing surface treatment on the profile to obtain a watch material.

4. The preparation method according to claim 3, characterized in that: In the S1, the melting includes firstly keeping the temperature at 650-720°C for 0.5-1h, and then keeping the temperature at 720-800°C for 0.5-1h.

5. The preparation method according to claim 3, characterized in that: In the S2, the refining temperature is 720-750°C and the holding time is 0.5-1h.

6. The preparation method according to claim 3, characterized in that: In the above-mentioned S3, the casting method includes a hot top method or an oil-gas sliding method.

7. The preparation method according to claim 3, characterized in that: In the above-mentioned S4, the homogenization treatment includes firstly keeping the temperature at 350-450°C for 3-6 hours and then keeping the temperature at 500-580°C for 4-8 hours; the extrusion speed of the extrusion molding is 1-10 m / min.

8. The preparation method according to claim 3, characterized in that: In the S4, the solution treatment includes keeping at 380-400°C for 3-6h; the aging treatment includes first heating to 150-170°C at 1-2°C / min and keeping at 3-6h, then heating to 170-190°C at 0.5-1°C / min and keeping at 4-8h, and cooling to below 40°C with strong wind.

9. The preparation method according to claim 3, characterized in that: In the above-mentioned S5, the surface treatment includes one or more of polishing, wire drawing, and anodizing.