Aluminum alloy profile for hot forging control arm and machining method and application of aluminum alloy profile
Through hot extrusion processing and T6 heat treatment of Al-Mg-Si alloy materials, combined with low-pressure vacuum casting and gradient heating technology, the problems of low processing efficiency and coarse-grained rings of aluminum alloy control arms in automobile suspension systems are solved, and high strength is achieved and efficient production of finished products.
Patent Information
- Application Number
- CN202410783837.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
The processing cycle of the aluminum alloy control arms in the existing automobile suspension system is long, the efficiency is low, the material utilization rate and the yield are low, and multiple forgings are required during the processing, resulting in the generation of coarse grain rings.
Al-Mg-Si alloy material is used, hot extrusion processing is performed after casting, combined with T6 heat treatment to reduce the flattening and bending process, low-pressure vacuum casting and gradient heating technology are used, and a profiling mold is designed to improve the density and strength of the finished product. .
It achieves high strength and low coarse grain rings of aluminum alloy profiles, improves processing efficiency and yield, reduces production costs, and improves the overall performance of aluminum alloys.
Smart Images

Figure CN118756006A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of processing of deformed aluminum alloy for automobiles, in particular to an aluminum alloy profile for hot forging control arms and a processing method and application thereof. Background Art
[0002] The automobile suspension system is an important assembly in modern automobiles, which has a great influence on the driving smoothness and handling stability of the automobile. As the guiding and force transmission element of the automobile suspension system, the control arm (also called the swing arm) transmits various forces acting on the wheel to the body, while ensuring that the wheel moves along a certain trajectory. The control arm elastically connects the wheel and the body through a ball joint or a bushing. With the continuous development of the automobile industry, the requirements for lightweight automobiles are getting higher and higher, and the use of lightweight aluminum alloys instead of steel and cast iron in automobiles is becoming more and more widespread.
[0003] Aluminum alloy control arms are key components of automobile suspension systems. They have complex shapes and are usually forged from hot extruded aluminum alloy round bars. Common processing procedures are: round bar cutting → heating → roll forging → flattening and bending → secondary heating → pre-forging, final forging → T6 heat treatment. In this process, the blank needs to be heated twice, which results in a long processing cycle and low efficiency. In addition, the material undergoes multiple forgings, resulting in low utilization and yield rates. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an aluminum alloy profile for hot forged control arms and a processing method and application thereof. The aluminum alloy profile is an Al-Mg-Si alloy, which is obtained by melting and casting → hot extrusion. It has excellent comprehensive performance and can well meet the requirements of good density, high strength, and suppression of coarse grain rings of aluminum alloy for hot forged control arms.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:
[0006] In a first aspect, an embodiment of the present invention provides an aluminum alloy profile for a hot forged control arm, comprising the following components, measured in weight percentage: Si 1.05%-1.25%, Fe<0.3%, Cu<0.1%, Mn 0.50%-0.65%, Mg 0.70%-0.95%, Cr 0.13%-0.20%, Ni<0.05%, Zn<0.05%, Ti<0.05%, and the balance is Al, wherein the total amount of Mn and Cr is 0.70-0.80%, and by mass ratio, Mg / Si is 0.5-0.9.
[0007] Furthermore, the following components are included in weight percentage: Si 1.08%-1.22%, Fe 0.18%-0.25%, Cu 0.02%-0.06%, Mn 0.56%-0.62%, Mg 0.78%-0.92%, Cr 0.14%-0.18%, Ni<0.05%, Zn<0.05%, Ti<0.05%, and the balance is Al.
[0008] In a second aspect, an embodiment of the present invention provides a method for processing the aluminum alloy profile for hot forging a control arm according to the first aspect, comprising the following steps:
[0009] (1) Melting:
[0010] (1.1) According to the lower limit of chemical composition, aluminum ingots, aluminum-silicon master alloys and recycled materials of the same series of alloys are added to the smelting furnace, heated and melted to a temperature of more than 750°C, fully stirred and slag removed;
[0011] (1.2) Take samples for chemical component analysis, add aluminum-silicon master alloy, iron agent, aluminum-copper master alloy, manganese agent, magnesium ingot, and chromium agent according to the median value of the chemical components, close the furnace door and keep warm for 10-20 minutes, stir thoroughly again and remove slag;
[0012] (1.3) After the chemical composition test is qualified, the aluminum liquid temperature is adjusted to 760-780℃ for refining, and a sodium-free particle refining agent is used, with a dosage of 1.5-2.0kg / t·Al, and the refining gas is argon, with an argon pressure of 0.35±0.05MPa, and the refining time is 30-35 minutes;
[0013] (1.4) After refining, remove the scum on the surface of the aluminum liquid, evenly sprinkle the sodium-free covering agent on the surface of the aluminum liquid, let it stand for 20-60 minutes, and then start casting after the standing time;
[0014] (2) Casting:
[0015] Aluminum alloy casting rods are obtained by casting using a low-pressure vacuum casting system. The casting speed is 40±2mm / min, and the casting water flow rate of a single mold is 16±5m 3 / h, casting crystal height: 85±3mm;
[0016] (3) Homogenization
[0017] After removing the head and tail of the cast rods that are unqualified and scrapped, the cast rods are homogenized at a temperature of 500-520°C, a holding time of 8-8.2 hours, and a cooling method of water cooling.
[0018] (4) Cutting and peeling:
[0019] (4.1) Cut the cast bars into multiple lengths, with the cutting length ranging from 1400 to 1700 mm, depending on the profile delivery length agreed with the customer;
[0020] (4.2) peeling the obtained short cast rods, and the outer diameter of the cast rods after peeling is 515-517 mm;
[0021] (5) Extrusion:
[0022] (5.1) Preheat the extrusion die barrel and die. The preheating temperature of the die barrel is 435±5℃ and the preheating temperature of the die is 480±5℃;
[0023] (5.2) The cast rod is heated and forward extruded. The temperature of the cast rod is 520±10°C at the head, 515±10°C in the middle, and 510±10°C at the tail. The extrusion speed is 1.0-3.0 m / min. The cooling method is air cooling to obtain an aluminum alloy profile.
[0024] Furthermore, after the aluminum alloy profile obtained by extrusion is subjected to T6 heat treatment, the tensile strength is ≥410MPa, the yield strength is ≥390MPa, the elongation is ≥10%, and the hardness is ≥HB115;
[0025] The relevant parameters for T6 heat treatment are as follows:
[0026] Vertical quenching process: 550±5℃, heat preservation 2±0.2h, metal temperature control;
[0027] Artificial aging process: 175±5℃, insulation 8±0.5h, metal temperature control.
[0028] Furthermore, the melting temperature in step (1.1) is 750-780° C., and mechanical stirring and electromagnetic stirring are used for sufficient stirring, the mechanical stirring depth is 400-600 mm, the mechanical stirring time is 10-15 minutes, and the electromagnetic stirring time is 30-35 minutes.
[0029] Furthermore, during the extrusion process in step (5), the shape of the aluminum alloy profile is designed according to the final forging shape of the forged control arm.
[0030] In the third aspect, an embodiment of the present invention provides an application of an aluminum alloy profile for a hot forged control arm. The aluminum alloy profile obtained in the second aspect is used to forge a control arm. After the prepared control arm undergoes T6 heat treatment, the tensile strength is ≥360MPa, the yield strength is ≥340MPa, the elongation is ≥10%, and the hardness is ≥HB115.
[0031] Furthermore, the relevant parameters during the T6 heat treatment are as follows:
[0032] Vertical quenching process: 535±5℃, insulation 2±0.2h, metal temperature control;
[0033] Artificial aging process: 175±5℃, insulation 8±0.5h, metal temperature control.
[0034] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0035] 1. The aluminum alloy profile of the present invention adopts a prefabricated profiling design, which can reduce the one-time flattening and bending process, reduce the forging deformation, better inhibit the generation of forging coarse grain rings, improve quality and reduce production costs.
[0036] 2. The present invention optimizes the chemical composition of the aluminum alloy, and the obtained aluminum alloy profile can obtain higher comprehensive properties, such as strength, hardness and structural uniformity, and no coarse grain ring.
[0037] 3. The aluminum alloy profile described in the present invention adopts sophisticated extrusion die design and precision manufacturing technology to obtain excellent external dimensions, which is conducive to improving the yield rate of subsequent forging and processing procedures.
[0038] 4. The cast rod for extrusion of the aluminum alloy profile described in the present invention is heated in a gradient along the extrusion direction to achieve constant speed extrusion and keep the outlet temperature stable, thereby making the microstructure and performance of the aluminum alloy profile more stable and consistent. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic diagram of the cross-sectional structure of the aluminum alloy profile in Example 1 of the present invention.
[0040] Figure 2 This is a low-magnification microstructure diagram of the aluminum alloy profile in T6 state in Example 1 of the present invention.
[0041] Figure 3-4 It is a low-magnification microstructure diagram of a local position of the aluminum alloy profile in Example 1 of the present invention.
[0042] Figure 5-6 This is a high-magnification microstructure diagram of the edge of the aluminum alloy profile in Example 1 of the present invention.
[0043] Figure 7-8 This is a high-magnification microstructure diagram of the core position of the aluminum alloy profile in Example 1 of the present invention.
[0044] Fig. 9 This is a picture of the finished product of the aluminum alloy profile after forging in Example 1 of the present invention. Among them, a, b, c, and d are the sampling positions of its mechanical properties respectively. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0046] Example 1
[0047] An aluminum alloy profile for a hot forged control arm comprises the following components by weight percentage: 1.19% Si, 0.218% Fe, 0.038% Cu, 0.594% Mn, 0.807% Mg, 0.167% Cr, 0.0039% Ni, 0.0048% Zn, 0.0297% Ti, and the balance is Al.
[0048] The processing method of the aluminum alloy profile for hot forging control arm comprises the following steps:
[0049] (1) Melting:
[0050] (1.1) According to the lower limit of chemical composition, aluminum ingots, aluminum-silicon master alloys and recycled materials of the same series of alloys are added to the melting furnace, heated and melted to a temperature of more than 750°C, fully stirred and slag removed;
[0051] The melting temperature is 772°C.
[0052] The sufficient stirring is mechanical stirring plus electromagnetic stirring, the mechanical stirring depth is 400 mm, the mechanical stirring time is 12 minutes, and the electromagnetic stirring time is 35 minutes.
[0053] (1.2) Take samples for chemical component analysis, add aluminum-silicon master alloy, iron agent, aluminum-copper master alloy, manganese agent, magnesium ingot, and chromium agent according to the median value of the chemical components, close the furnace door and keep warm for 15 minutes, stir thoroughly again and remove slag;
[0054] (1.3) After the chemical composition test is qualified, the aluminum liquid temperature is adjusted to 770°C for refining, and a sodium-free particle refining agent is used, with a dosage of 1.78 kg / t·Al, and the refining gas is argon, with an argon pressure of 0.35 MPa, and the refining time is 35 minutes;
[0055] (1.4) After refining, remove the scum on the surface of the aluminum liquid, evenly sprinkle the sodium-free covering agent on the surface of the aluminum liquid, let it stand for 45 minutes, and then start casting after the standing time;
[0056] (2) Casting:
[0057] The low pressure vacuum casting system is used for casting. Aluminum alloy casting rod, casting speed: 40mm / min, casting water flow: 16m 3 / h / mould, casting crystal height: 85mm, casting rod length 5970mm;
[0058] (3) Homogenization treatment:
[0059] After removing 550mm from the head of the cast rod and 250mm from the tail, a homogenization treatment is performed. The homogenization treatment temperature is 510°C, the insulation time is 8 hours, and the cooling method is water cooling.
[0060] (4) Cutting and peeling:
[0061] (4.1) Cut the cast rod into multiple lengths, with a cutting length of 1700 mm;
[0062] (4.2) The obtained short cast rods are peeled, and the outer diameter of the cast rods after peeling is 515 mm.
[0063] (5) Extrusion:
[0064] (5.1) Preheat the extrusion die barrel and die to 435°C and 480°C respectively.
[0065] (5.2) Heat the cast rod and perform forward extrusion. The temperature of the cast rod head is 521℃, the temperature of the middle part is 517℃, the temperature of the tail is 508℃, the extrusion speed is 3.0mm / s, the discharge speed is 1.2m / min, and the cooling method is air cooling. The shape of the aluminum alloy profile is designed according to the final forging shape of the forged control arm. The structure is shown in Figure 1 shown.
[0066] The aluminum alloy profile is integrally formed by extruding the aluminum alloy material as a whole through a mold. The cross-section of the aluminum alloy profile includes a first end 1, a second end 2 and a third end 3. The third end 3 is connected to the first end 1 and the second end 2 respectively. A V-shaped groove 4 is provided between the first end 1 and the second end 2. The opening of the V-shaped groove 4 is located between the free ends of the first end 1 and the second end 2. The bottom of the V-shaped groove 4 is connected to the third end 3.
[0067] The first end 1, the second end 2 and the third end 3 are respectively located at three vertices of a virtual triangle. The virtual triangle is one of an equilateral triangle, an isosceles triangle or an unequal-sided triangle.
[0068] The third end portion 3 is connected to the first end portion 1 and the second end portion 2 respectively through a plurality of arc surfaces of unequal diameters.
[0069] The free end sizes of the first end 1 and the second end 2 are larger than the size of the connecting portion 5 between the first end 1, the second end 2 and the third end 3. The free end sizes of the first end 1 and the second end 2 are the same or different.
[0070] The mechanical properties and hardness of the aluminum alloy profile after T6 heat treatment in Example 1 of the present invention are shown in Table 1 below; the macrostructure of the aluminum alloy profile after T6 heat treatment is shown in Figure 2 As shown, from Figure 2 It can be seen that the macrostructure of the aluminum alloy profile T6 state in the embodiment of the present invention is dense and uniform, and there is no coarse grain ring on the edge.
[0071] Figure 3-4 is a low-magnification microstructure diagram of a local position of the aluminum alloy profile in Example 1 of the present invention. Figure 3-4 It can be seen that the macrostructure of the local part of the aluminum alloy is dense and uniform, and there is no coarse grain ring at the edge.
[0072] Figure 5-6 is a high-magnification microstructure diagram of the edge of the aluminum alloy profile in Example 1 of the present invention. Figure 5-6 It can be seen that the structure at the edge of the aluminum alloy is dense and uniform, and there is no coarse grain ring at the edge.
[0073] Figure 7-8 is a high-magnification microstructure diagram of the core of the aluminum alloy profile in Example 1 of the present invention. Figure 7-8 It can be seen that the structure at the core of the aluminum alloy profile is dense and uniform.
[0074] Table 1 Mechanical properties and hardness of the aluminum alloy profile after T6 heat treatment in Example 1 of the present invention
[0075]
[0076] It can be seen from Table 1 that after the aluminum alloy profile in Example 1 is subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥410 MPa, yield strength ≥390 MPa, elongation ≥10%, and hardness ≥HB115.
[0077] The aluminum alloy profile of the present invention is forged into a control arm. Fig. 9 As shown in Table 2, after T6 heat treatment, the mechanical properties and hardness are tested.
[0078] Table 2 Mechanical properties and hardness of aluminum alloy profiles forged into control arms and subjected to T6 heat treatment in Example 1 of the present invention
[0079] state Tensile strength(MPa) Yield strength (MPa) Elongation / % Hardness / HB Position a 387 369 11.0 118 Position b 394 376 10.7 122 Position c 384 361 11.7 119 Position d 389 363 10.8 120
[0080] It can be seen from Table 2 that after the aluminum alloy profile in Example 1 is forged into a control arm and subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥360MPa, yield strength ≥340MPa, elongation ≥10%, and hardness ≥HB115.
[0081] Example 2
[0082] An aluminum alloy profile for a hot forged control arm comprises the following components by weight percentage: 1.20% Si, 0.211% Fe, 0.0328% Cu, 0.600% Mn, 0.802% Mg, 0.173% Cr, 0.0034% Ni, 0.0148% Zn, 0.0439% Ti, and the balance is Al.
[0083] The processing method of the aluminum alloy profile for hot forging control arm comprises the following steps:
[0084] (1) Melting:
[0085] (1.1) According to the lower limit of chemical composition, aluminum ingots, aluminum-silicon master alloys and recycled materials of the same series of alloys are added to the melting furnace, heated and melted to a temperature of more than 750°C, fully stirred and slag removed;
[0086] The melting temperature is 765℃.
[0087] The sufficient stirring is mechanical stirring plus electromagnetic stirring, the mechanical stirring depth is 500 mm, the mechanical stirring time is 14 minutes, and the electromagnetic stirring time is 32 minutes.
[0088] (1.2) Take samples for chemical component analysis, add aluminum-silicon master alloy, iron agent, aluminum-copper master alloy, manganese agent, magnesium ingot, and chromium agent according to the median value of the chemical components, close the furnace door and keep warm for 18 minutes, stir thoroughly again and remove slag;
[0089] (1.3) After the chemical composition test is qualified, the aluminum liquid temperature is adjusted to 770°C for refining, and a sodium-free particle refining agent is used, with a dosage of 1.62 kg / t·Al, and the refining gas is argon, with an argon pressure of 0.37 MPa, and the refining time is 31 minutes;
[0090] (1.4) After refining, remove the scum on the surface of the aluminum liquid, evenly sprinkle the sodium-free covering agent on the surface of the aluminum liquid, let it stand for 48 minutes, and then start casting after the standing time;
[0091] (2) Casting:
[0092] The low pressure vacuum casting system is used for casting. Aluminum alloy casting rod, casting speed: 42mm / min, casting water flow: 21m 3 / h / mould, casting crystal height: 88mm, casting rod length 5840mm;
[0093] (3) Homogenization treatment:
[0094] After removing 565mm from the head of the cast rod and 260mm from the tail, a homogenization treatment is performed. The homogenization treatment temperature is 500°C, the insulation time is 8.2 hours, and the cooling method is water cooling.
[0095] (4) Cutting and peeling:
[0096] (4.1) Cut the cast rod into multiple lengths, with a cutting length of 1640 mm;
[0097] (4.2) The obtained short cast rods are peeled, and the outer diameter of the cast rods after peeling is 516 mm.
[0098] (5) Extrusion:
[0099] (5.1) Preheat the extrusion die barrel and die to 440°C and 485°C respectively.
[0100] (5.2) Heat the cast rod and perform forward extrusion. The temperature of the cast rod head is 524℃, the temperature of the middle part is 514℃, the temperature of the tail is 507℃, the extrusion speed is 3.7mm / s, the discharge speed is 1.5m / min, and the cooling method is air cooling. The shape of the aluminum alloy profile is designed according to the final forging shape of the forged control arm. The structure is shown in Figure 1 shown.
[0101] After the aluminum alloy profile of the present invention is subjected to T6 heat treatment, the mechanical properties and hardness thereof are shown in Table 3 below.
[0102] Table 3 Mechanical properties and hardness of the aluminum alloy profiles after T6 heat treatment in Example 2 of the present invention
[0103]
[0104] It can be seen from Table 3 that after the aluminum alloy profile in Example 2 is subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥410 MPa, yield strength ≥390 MPa, elongation ≥10%, and hardness ≥HB115.
[0105] The aluminum alloy profile of the present invention is forged into a control arm. Fig. 9 As shown in Table 4, after T6 heat treatment, the mechanical properties and hardness are tested.
[0106] Table 4 Mechanical properties and hardness of aluminum alloy profiles forged into control arms and subjected to T6 heat treatment in Example 2 of the present invention
[0107]
[0108]
[0109] It can be seen from Table 4 that after the aluminum alloy profile in Example 2 is forged into a control arm and subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥360MPa, yield strength ≥340MPa, elongation ≥10%, and hardness ≥HB115.
[0110] Example 3
[0111] An aluminum alloy profile for a hot forged control arm comprises the following components by weight: 1.17% Si, 0.221% Fe, 0.0260% Cu, 0.606% Mn, 0.817% Mg, 0.166% Cr, 0.0028% Ni, 0.007% Zn, 0.0370% Ti, and the balance is Al.
[0112] The processing method of the aluminum alloy profile for hot forging control arm comprises the following steps:
[0113] (1) Melting:
[0114] (1.1) According to the lower limit of chemical composition, aluminum ingots, aluminum-silicon master alloys and recycled materials of the same series of alloys are added to the melting furnace, heated and melted to a temperature of more than 750°C, fully stirred and slag removed;
[0115] The melting temperature is 768℃.
[0116] The sufficient stirring is mechanical stirring plus electromagnetic stirring, the mechanical stirring depth is 600 mm, the mechanical stirring time is 13 minutes, and the electromagnetic stirring time is 31 minutes.
[0117] (1.2) Take samples for chemical component analysis, add aluminum-silicon master alloy, iron agent, aluminum-copper master alloy, manganese agent, magnesium ingot, and chromium agent according to the median value of the chemical components, close the furnace door and keep warm for 13 minutes, stir thoroughly again and remove slag;
[0118] (1.3) After the chemical composition test is qualified, the aluminum liquid temperature is adjusted to 770°C for refining, and a sodium-free particle refining agent is used, with a dosage of 1.89 kg / t·Al, and the refining gas is argon, with an argon pressure of 0.32 MPa, and the refining time is 32 minutes;
[0119] (1.4) After refining, remove the scum on the surface of the aluminum liquid, evenly sprinkle the sodium-free covering agent on the surface of the aluminum liquid, let it stand for 56 minutes, and then start casting after the standing time;
[0120] (2) Casting:
[0121] The low pressure vacuum casting system is used for casting. Aluminum alloy casting rod, casting speed: 38mm / min, casting water flow: 11m 3 / h / mould, casting crystal height: 82mm, casting rod length 6890mm;
[0122] (3) Homogenization treatment:
[0123] After removing 590mm from the head of the cast rod and 280mm from the tail, a homogenization treatment is performed. The homogenization treatment temperature is 520℃, the insulation time is 7.8 hours, and the cooling method is water cooling.
[0124] (4) Cutting and peeling:
[0125] (4.1) Cut the cast rod into multiple lengths, with a cutting length of 1480 mm;
[0126] (4.2) The obtained short cast rods are peeled, and the outer diameter of the cast rods after peeling is 517 mm.
[0127] (5) Extrusion:
[0128] (5.1) Preheat the extrusion die barrel and die. The preheating temperature of the die barrel is 430°C and the preheating temperature of the die is 475°C.
[0129] (5.2) Heat the cast rod and perform forward extrusion. The temperature of the cast rod head is 518℃, the temperature of the middle part is 512℃, the temperature of the tail is 511℃, the extrusion speed is 4.5mm / s, the discharge speed is 1.8m / min, and the cooling method is air cooling. The shape of the aluminum alloy profile is designed according to the final forging shape of the forged control arm. The structure is shown in Figure 1 shown.
[0130] After the aluminum alloy profile of the present invention is subjected to T6 heat treatment, the mechanical properties and hardness thereof are shown in Table 5 below.
[0131] Table 5 Mechanical properties and hardness of the aluminum alloy profiles after T6 heat treatment in Example 3 of the present invention
[0132]
[0133] It can be seen from Table 5 that after the aluminum alloy profile in Example 3 is subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥410 MPa, yield strength ≥390 MPa, elongation ≥10%, and hardness ≥HB115.
[0134] The aluminum alloy profile of the present invention is forged into a control arm. Fig. 9 As shown in Table 6, after T6 heat treatment, the mechanical properties and hardness are tested.
[0135] Table 6 Mechanical properties and hardness of aluminum alloy profiles forged into control arms and subjected to T6 heat treatment in Example 3 of the present invention
[0136] state Tensile strength(MPa) Yield strength (MPa) Elongation / % Hardness / HB Position a 387 364 11.5 125 Position b 390 378 10.7 121 Position c 385 369 11.0 123 Position d 386 362 11.9 124
[0137] It can be seen from Table 6 that after the aluminum alloy profile in Example 3 is forged into a control arm and subjected to T6 heat treatment, its mechanical properties and hardness meet the following requirements: tensile strength ≥360MPa, yield strength ≥340MPa, elongation ≥10%, and hardness ≥HB115.
[0138] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. An aluminum alloy profile for hot forging control arm, characterized in that: Calculated by weight percentage, it includes the following components: Si 1.05%-1.25%, Fe <0.3%, Cu <0.1%, Mn 0.50%-0.65%, Mg 0.70%-0.95%, Cr 0.13%-0.20%, Ni <0.05%, Zn <0.05%, Ti <0.05%, and the balance is Al, of which the total amount of Mn and Cr is 0.70-0.80%, and by mass ratio, Mg / Si is 0.5-0.
9.
2. The aluminum alloy profile for hot forging control arm according to claim 1, characterized in that: Calculated by weight percentage, it includes the following components: Si 1.08%-1.22%, Fe 0.18%-0.25%, Cu 0.02%-0.06%, Mn 0.56%-0.62%, Mg0.78%-0.92%, Cr 0.14%-0.18%, Ni<0.05%, Zn<0.05%, Ti<0.05%, and the balance is Al.
3. The processing method of the aluminum alloy profile for hot forging control arm according to claim 1 or 2, characterized in that: The following steps are involved: (1) Melting: (1.1) According to the lower limit of chemical composition, add aluminum ingots, aluminum-silicon master alloys and recycled materials of the same series of alloys into the smelting furnace, heat and melt them to a temperature of more than 750°C, stir them thoroughly and remove the slag; (1.2) Take samples for chemical component analysis, add aluminum-silicon master alloy, iron agent, aluminum-copper master alloy, manganese agent, magnesium ingot, and chromium agent according to the median value of the chemical components, close the furnace door and keep warm for 10-20 minutes, stir thoroughly again and remove slag; (1.3) After the chemical composition test is qualified, adjust the aluminum liquid temperature to 760-780℃ for refining, use sodium-free particle refining agent, the dosage is 1.5-2.0 kg / t·Al, the refining gas is argon, the argon pressure is 0.35±0.05MPa, and the refining time is 30-35 minutes; (1.4) After refining, remove the scum on the surface of the aluminum liquid, evenly sprinkle the sodium-free covering agent on the surface of the aluminum liquid, let it stand for 20-60 minutes, and then start casting; (2) Casting: Aluminum alloy casting rods are obtained by casting using a low-pressure vacuum casting system. The casting speed is 40±2 mm / min and the casting water flow rate of a single mold is 16±5m 3 / h, casting crystal height: 85±3mm; (3) Homogenization treatment After removing the head and tail of the cast rods that are unqualified and scrapped, the cast rods are homogenized at a temperature of 500-520°C, a holding time of 8-8.2 hours, and a cooling method of water cooling. (4) Cutting and peeling: (4.1) Cut the cast bars into multiple lengths, with the cutting length ranging from 1400 to 1700 mm, depending on the profile delivery length agreed with the customer; (4.2) peeling the obtained short cast rods, and the outer diameter of the cast rods after peeling is 515-517 mm; (5) Extrusion: (5.1) Preheat the extrusion die barrel and die. The preheating temperature of the die barrel is 435±5℃, and the preheating temperature of the die is 480±5℃; (5.2) The cast rod is heated and forward extruded. The temperature of the cast rod is 520±10°C at the head, 515±10°C in the middle, and 510±10°C at the tail. The extrusion speed is 1.0-3.0 m / min. The cooling method is air cooling to obtain an aluminum alloy profile.
4. The method for processing the aluminum alloy profile for hot forging control arm according to claim 3, characterized in that: After T6 heat treatment, the aluminum alloy profile obtained by extrusion has a tensile strength of ≥410MPa, a yield strength of ≥390MPa, an elongation of ≥10%, and a hardness of ≥HB115; The relevant parameters for T6 heat treatment are as follows: Vertical quenching process: 550±5℃, holding time 2±0.2 h, metal temperature control; Artificial aging process: 175±5℃, insulation 8±0.5h, metal temperature control.
5. The method for processing the aluminum alloy profile for hot forging control arm according to claim 3, characterized in that: The melting temperature in step (1.1) is 750-780°C. Mechanical stirring and electromagnetic stirring are used for full stirring. The mechanical stirring depth is 400-600 mm. The mechanical stirring time is 10-15 minutes and the electromagnetic stirring time is 30-35 minutes.
6. The method for processing the aluminum alloy profile for hot forging control arm according to claim 3, characterized in that: During the extrusion process in step (5), the shape of the aluminum alloy profile is designed according to the final forging shape of the forged control arm.
7. An application of an aluminum alloy profile for hot forging control arm, characterized in that: The aluminum alloy profile obtained in claim 3 is used for forging a control arm. After the control arm is subjected to T6 heat treatment, the tensile strength is ≥360MPa, the yield strength is ≥340MPa, the elongation is ≥10%, and the hardness is ≥HB115.
8. The use of the aluminum alloy profile for hot forging control arm according to claim 7, characterized in that: The relevant parameters during the T6 heat treatment are as follows: Vertical quenching process: 535±5℃, holding time 2±0.2 h, metal temperature control; Artificial aging process: 175±5℃, insulation 8±0.5h, metal temperature control.