Micro-alloying method for wind power steel in smelting process
By adding self-reducing vanadium slag into the ladle and controlling the use of argon gas and lime, the recovery rate of vanadium in the vanadium slag is improved, solving the problems of long process, high cost and waste of resources in the existing process, and realizing efficient vanadium production. Slag recycling.
Patent Information
- Application Number
- CN202411196450.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-10-11
AI Technical Summary
The existing vanadium extraction process from vanadium slag has a long process, complex process, high cost and low resource utilization rate, resulting in serious waste of resources.
Add self-reducing vanadium slag into the ladle and reduce it by blowing argon gas. Control the flow and temperature of the argon gas, combined with the use of lime and aluminum, carry out the refining process of molten steel and increase the recovery rate of vanadium in the vanadium slag.
The vanadium extraction process is shortened, the production cost is reduced, the recovery rate of vanadium slag is increased, the recovery rate reaches more than 80%, and the pollution problem is reduced.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing equipment and relates to a micro-alloying method in a smelting process of steel for wind power generation. Background Art
[0002] Steel plates for wind power are mainly used to make wind power towers. Currently, the towers are mainly made of Q390NE and Q420NE medium and thick plates using the bending and welding process. Since most of the towers are located in the northern region, in addition to strength, plasticity, and welding performance indicators, the material is also required to have the ability to prevent low-temperature brittle fracture and resist low-temperature impact loads.
[0003] When there is a certain amount of vanadium, carbon and nitrogen in steel materials, vanadium precipitates will be produced in the matrix of the steel. These precipitates will promote the nucleation of intracrystalline ferrite, and their particles can pin the grain boundaries, thereby refining the ferrite grains. At the same time, the second phase precipitated by vanadium at low temperatures is mainly formed by interphase precipitation, which is more uniform, fine and dispersed. It can play a significant role in precipitation strengthening, significantly improve the strength, toughness, plasticity, ductility and welding performance of steel, prevent low-temperature brittle fracture and improve the ability to withstand low-temperature impact loads.
[0004] Vanadium in nature is mainly found in vanadium-titanium magnetite. The iron and vanadium in vanadium-titanium magnetite cannot be enriched and separated by physical separation methods. Generally, vanadium slag needs to be produced through the process of molten iron blowing vanadium, that is, the vanadium-titanium magnetite concentrate is smelted in a blast furnace to obtain vanadium-containing molten iron, and the vanadium-containing pig iron is further oxidized and blown to obtain vanadium slag with a V2O5 content of 12%-16%. Vanadium slag is the raw material for vanadium extraction. After a series of vanadium extraction methods, vanadium-containing alloys of a certain purity and shape are obtained, which are then used for vanadium alloying in the steel production process. The main methods for extracting vanadium from vanadium slag are: sodium oxidation roasting to extract vanadium, calcium oxidation roasting to extract vanadium, salt-free oxidation roasting to extract vanadium, non-roasting pressure leaching, direct oxidation extraction of vanadium from molten vanadium slag, and vanadium extraction from waste catalysts. However, these methods have the problems of long processes, complex processes, serious pollution in the production process, and high production costs.
[0005] The invention patent with publication number CN 113122678 A provides "a smelting method for vanadium-enriched steelmaking using vanadium slag" and proposes a V alloying scheme of converter steelmaking deoxidation - LF furnace heating - adding vanadium slag and alloy alloying - recovering vanadium slag - ladle furnace refining furnace treatment - continuous casting. The method is used for vanadium-enriched steelmaking, which can well solve the problems of long process flow, complex process, serious pollution in the production process and high production process cost of vanadium slag extraction process, but its recovery rate is only 65-80%, and there are problems of resource waste and low utilization rate. Summary of the invention
[0006] The purpose of the present invention is to provide a method for microalloying in the smelting process of steel for wind power generation in view of the problems of resource waste and low utilization rate in the existing methods in the background technology.
[0007] To this end, the present invention adopts the following technical solutions: A method for microalloying in a steel smelting process for wind power generation, comprising the following steps: (1) During the steelmaking process of the converter, the self-reducing vanadium slag is added into the ladle along with the steel flow. The amount of self-reducing vanadium slag added is 7-12 kg / t and argon is continuously blown. The argon bottom blowing flow rate is 20-30 m 3 / h; (2) After steel tapping is completed, adjust the bottom blowing argon flow rate to 1-5m 3 / h, control the aluminum content in the molten steel to 300-400ppm, blow argon for 3-5 minutes before transferring the molten steel to the ladle refining furnace; (3) Add lime to the ladle refining furnace, control the slag basicity of the ladle furnace to 1.0-2.0, and blow argon into the ladle refining furnace for 1-3 minutes at a flow rate of 20-30m 3 / h, so that the added lime can be completely spread on the surface of the slag; (4) Raise the temperature of molten steel for 20-30 minutes to 1580-1600℃. During the heating process, the arc current of the ladle refining furnace electrode is 20000-25000A, the voltage is 120V, and argon is blown from the bottom. The flow rate of argon is 10-20m 3 / h, after heating, adjust the bottom blowing argon flow rate to 1-5m 3 / h.
[0008] Furthermore, the percentage of each component in the self-reducing vanadium slag in step (1) is: SiO 2 :30-40%, CaO: 10-15%, C: 5-10%, SiC: 10-20%, V 2 O 5 :5-10%,MnO:6-10%,Fe 2 O 3 : 10-20%.
[0009] Furthermore, in step (1), the tapping temperature of the converter is 1620-1650°C, and the slag volume of the converter is less than 50 mm.
[0010] Furthermore, in the step (2), the aluminum content in the molten steel is controlled by feeding aluminum wire.
[0011] Furthermore, in the step (2), when the molten steel is transferred to the ladle refining furnace, the inlet temperature of the molten steel is greater than 1530°C.
[0012] The beneficial effects of the present invention are as follows: the vanadium in the vanadium slag can be directly reduced into molten steel through the present invention, which greatly shortens the process of the traditional vanadium extraction process, saves the cost of the vanadium extraction process, and alleviates the problem of serious pollution in the production process; the recovery rate of vanadium in the vanadium slag is improved, and the vanadium recovery rate after smelting is completed can reach more than 80%. DETAILED DESCRIPTION
[0013] The present invention is described in detail below in conjunction with embodiments: The production of wind power panel Q420NE by 50t converter is taken as an example to illustrate the actual implementation process and effect of the present invention, and the molten steel of B224103875, B224103936 and B224103987 are used for specific description.
[0014] Example 1 (1) During the converter tapping process, the self-reducing vanadium slag is added into the ladle along with the steel flow. The temperature of the molten steel during converter tapping is 1621°C, the slag volume during converter tapping is 40 mm, and the composition of the molten steel during tapping is shown in Table 1: Table 1 In this implementation, the amount of self-reducing vanadium slag added was 8.5 kg / t and argon was continuously blown, with an argon bottom blowing flow rate of 20 m 3 / h, the percentages of various components in the self-reducing vanadium slag are shown in Table 2: Table 2 When adding molten steel into the ladle, argon is continuously blown into the molten steel, and the argon bottom blowing flow rate is 20-30m 3 / h.
[0015] (2) After steel tapping is completed, the ladle is transferred to the argon blowing station and the bottom argon blowing flow rate is adjusted to 2m 3 / h, the aluminum content in the molten steel is controlled to be 400ppm by feeding 180m of aluminum wire, and the molten steel is transferred to the ladle refining furnace after blowing argon for 3 minutes. When the molten steel is transferred to the ladle refining furnace, the inlet temperature of the molten steel is 1540℃.
[0016] (3) Add lime to the ladle refining furnace, control the slag basicity of the ladle furnace to 2.0, and blow argon into the ladle refining furnace for 1 minute at a flow rate of 20m 3 / h, so that the added lime can be completely spread on the surface of the slag.
[0017] (4) Raise the temperature of molten steel for 20 minutes to 1590°C. During the heating, the arc current of the ladle refining furnace electrode is 22000A, the voltage is 120V, and the bottom blowing flow rate is 10m 3 / h, after heating, adjust the bottom blowing argon to 1m 3 / h, after refining, the molten steel is transferred to the continuous casting machine for pouring. After refining, the composition of the finished molten steel is shown in Table 3: Table 3 The amount of vanadium slag used in the B224103875 ladle refining furnace process, the changes in the vanadium element in the molten steel, and the recovery rate of the vanadium element in the vanadium slag in the reducing slag after completion are shown in Table 4 below.
[0018] Table 4 Example 2 (1) During the converter tapping process, the self-reducing vanadium slag is added into the ladle along with the steel flow. The molten steel temperature is 1650°C during converter tapping, and the slag volume is 30 mm. The composition of the molten steel during tapping is shown in Table 5: Table 5 In this implementation, the amount of self-reducing vanadium slag added was 7.2 kg / t and argon was continuously blown, with an argon bottom blowing flow rate of 20 m 3 / h, the percentages of various components in the self-reducing vanadium slag are shown in Table 6: Table 6 When adding molten steel into the ladle, argon is continuously blown into the molten steel, and the argon bottom blowing flow rate is 20-30m 3 / h.
[0019] (2) After the steel is tapped, the ladle is transferred to the argon blowing station and the bottom argon blowing flow rate is adjusted to 5m 3 / h, the aluminum content in the molten steel is controlled to be 300ppm by feeding 140m of aluminum wire, and the molten steel is transferred to the ladle refining furnace after blowing argon for 1min. When the molten steel is transferred to the ladle refining furnace, the inlet temperature of the molten steel is 1550℃.
[0020] (3) Add lime to the ladle refining furnace, control the slag basicity of the ladle furnace to 1.0, and blow argon into the ladle refining furnace for 1 minute at a flow rate of 30m 3 / h, so that the added lime can be completely spread on the surface of the slag.
[0021] (4) Raise the temperature of molten steel for 30 minutes until the temperature reaches 1600°C. During the heating process, the arc current of the ladle refining furnace is 20000A, the voltage is 120V, and the bottom blowing flow rate is 20m 3 / h, after heating, adjust the bottom blowing argon to 5m 3 / h, after refining, the molten steel is transferred to the continuous casting machine for pouring. After refining, the composition of the finished molten steel is shown in Table 7: Table 7 The amount of vanadium slag used in the B224103936 ladle refining furnace process, the changes in the vanadium element in the molten steel and the recovery rate of the vanadium element in the vanadium slag in the reducing slag after completion are shown in Table 8 below.
[0022] Table 8 Example 3 (1) During the converter steel tapping process, the self-reducing vanadium slag is added into the ladle along with the steel flow. The temperature of the molten steel during converter steel tapping is 1644°C, the slag volume during converter steel tapping is 40 mm, and the composition of the molten steel during steel tapping is shown in Table 9: Table 9 In this embodiment, the amount of self-reducing vanadium slag added is 12kg / t and argon is continuously blown, and the argon bottom blowing flow rate is 20m 3 / h, the percentages of various components in the self-reducing vanadium slag are shown in Table 10: Table 10 When adding molten steel into the ladle, argon is continuously blown into the molten steel, and the argon bottom blowing flow rate is 20-30m 3 / h.
[0023] (2) After steel tapping is completed, the ladle is transferred to the argon blowing station and the bottom argon blowing flow rate is adjusted to 2m 3 / h, the aluminum content in the molten steel is controlled to be 350ppm by feeding 160m of aluminum wire, and the molten steel is transferred to the ladle refining furnace after blowing argon for 4 minutes. When the molten steel is transferred to the ladle refining furnace, the inlet temperature of the molten steel is 1550℃.
[0024] (3) Add lime to the ladle refining furnace, control the slag basicity of the ladle furnace to 1.5, and blow argon into the ladle refining furnace for 2 minutes at a flow rate of 25m 3 / h, so that the added lime can be completely spread on the surface of the slag.
[0025] (4) Raise the temperature of molten steel for 25 minutes to 1600°C. During the heating, the arc current of the ladle refining furnace electrode is 25000A, the voltage is 120V, and the bottom blowing flow rate is 15m 3 / h, after heating, adjust the bottom blowing argon to 3m 3 / h, after refining, the molten steel is transferred to the continuous casting machine for pouring. After refining, the composition of the finished molten steel is shown in Table 11: Table 11 The amount of vanadium slag used in the B224103987 ladle refining furnace process, the changes in the vanadium element in the molten steel and the recovery rate of the vanadium element in the reducing slag after completion are shown in Table 12 below.
[0026] Table 12 .
Claims
1. A method for microalloying in the smelting process of steel for wind power generation, characterized in that: The following steps are involved: (1) During the steelmaking process of the converter, the self-reducing vanadium slag is added into the ladle along with the steel flow. The amount of self-reducing vanadium slag added is 7-12 kg / t and argon is continuously blown. The argon bottom blowing flow rate is 20-30 m 3 / h; (2) After steel tapping is completed, adjust the bottom blowing argon flow rate to 1-5m 3 / h, control the aluminum content in the molten steel to 300-400ppm, blow argon for 3-5 minutes before transferring the molten steel to the ladle refining furnace; (3) Add lime to the ladle refining furnace, control the slag basicity of the ladle furnace to 1.0-2.0, and blow argon into the ladle refining furnace for 1-3 minutes at a flow rate of 20-30m 3 / h, so that the added lime can be completely spread on the surface of the slag; (4) Raise the temperature of molten steel for 20-30 minutes to 1580-1600℃. During the heating process, the arc current of the ladle refining furnace electrode is 20000-25000A, the voltage is 120V, and argon is blown from the bottom. The flow rate of argon is 10-20m 3 / h, after heating, adjust the bottom blowing argon flow rate to 1-5m 3 / h.
2. The method for microalloying in the smelting process of steel for wind power generation according to claim 1 is characterized in that: The percentages of the components in the self-reducing vanadium slag in step (1) are: SiO2: 30-40%, CaO: 10-15%, C: 5-10%, SiC: 10-20%, V2O5: 5-10%, MnO: 6-10%, Fe2O3: 10-20%.
3. The method for microalloying in the smelting process of steel for wind power generation according to claim 1 is characterized in that: In the step (1), the tapping temperature of the converter is 1620-1650° C., and the slag volume of the converter is less than 50 mm.
4. The method for microalloying in a steel smelting process for wind power generation according to claim 1 is characterized in that: In the step (2), the aluminum content in the molten steel is controlled by feeding aluminum wire.