Atmospheric plasma spraying method and thermal barrier coating

The thickness of alternating layers is controlled by the atmospheric plasma spraying method to prepare alternating multi-layer ceramic insulation layers, which solves the problem of excessive thickness of thermal barrier coatings, achieves excellent thermal resistance and insulation effects under high temperature conditions, and is suitable for aviation power turbines temperature rise requirement.

CN118756089AInactive Publication Date: 2024-10-11BEIJING GOLDEN WHEEL SPECIAL MACHINE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411005958.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The overall thickness of the existing thermal barrier coating is too large and difficult to control within 20 μm, and the change in heat conduction mode in high-temperature environments results in poor thermal radiation heat transfer suppression effect, making it difficult to meet the demand for increased temperatures in front of aerospace power turbines under high-temperature conditions. .

Method used

Using the atmospheric plasma spraying method, through the alternating layer thickness control step, the parameters of the feeding device, motion control device and spraying system are obtained, and combined with the information from the thickness feedback system, the thickness of each layer of material is adjusted to prepare alternating multi-layer ceramic insulation layers. Ensure the overall thickness and weight requirements of the coating, while improving thermal resistance and insulation effects.

Benefits of technology

It is possible to reduce the overall thickness of the alternating multi-layer ceramic insulation layer to meet the thickness and weight requirements while ensuring the thermal insulation performance. It also improves the heat reflection performance and reduces the thermal conductivity through the multi-layer structure to adapt to the heat under high temperature conditions. Radiant heat transfer requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756089A_ABST
    Figure CN118756089A_ABST
Patent Text Reader

Abstract

The invention provides an atmospheric plasma spraying method and a thermal barrier coating, relates to the technical field of thermal spraying, and aims to solve the problem that the overall thickness of the thermal barrier coating is too large. The atmosphere plasma spraying method comprises an alternating layer thickness control step, and in the alternating layer thickness control step, a first parameter of a feeding device, a second parameter of a motion control device, a third parameter of a spraying system and feedback information of a thickness feedback system are obtained, and the feeding device, the motion control device and the spraying system are controlled. The overall thickness of the thermal barrier coating can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal spraying, and in particular to an atmospheric plasma spraying method and a thermal barrier coating. Background Art

[0002] Atmosphere plasma spray (APS) is a surface treatment method that utilizes the high temperature and high energy effect of plasma flame to heat ceramic particles until they melt, and then spray the powder onto the substrate surface with the help of high-speed flame flow to form a coating. It has the advantages of mature technology, high deposition efficiency, high coating quality, and strong bonding force. However, in the conventional APS spraying process, the thickness of the ceramic layer is difficult to control within 20μm, and the thickness of the bonding layer is usually above 60μm, which makes the total thickness of the prepared film layer also mostly above 100μm, which makes the total mass of the coating relatively large, and is not suitable for devices with thickness restrictions on the coating and devices with high requirements for lightweight.

[0003] In addition, as the ambient temperature of thermal barrier coatings is increasing, single-structure thermal barrier coatings have gradually failed to meet the working conditions. When the ambient temperature is higher than 1100°C, the traditional zirconium oxide-based thermal barrier coating material is translucent, and its heat conduction mode gradually changes from phonon scattering to photon and electron conduction. The proportion of infrared thermal radiation increases. In order to meet the increasing demand for the temperature in front of more advanced aviation power turbines, thermal radiation heat transfer suppression is essential. At present, the development of high-emissivity and high-heat dissipation coating material systems, low-emission and high-thermal reflectivity coating material systems, multi-layer and multi-interface thermal reflection structures, and surface infrared radiation suppression coating systems are the main technical directions. The research and development of materials is extremely difficult, involving multiple dimensions such as light, electricity, and heat, as well as various optimizations of material composition and crystal structure. At present, Yb-doped modified, Pt-doped modified, and Al-doped modified coating materials have been developed to reduce the thermal conductivity of coatings under high-temperature conditions with a high proportion of thermal radiation, but they are still in the laboratory stage. In this context, how to use the thermal conductivity characteristics of different heterogeneous materials to prepare multi-layer and multi-interface thermal reflection structures has become the focus of industry research. Although the interface can increase the thermal reflection effect, increase the light and electron attenuation path, and thus reduce thermal conductivity, as mentioned above, the low-cost APS technology has core technical problems such as the thick thickness of the multiple alternating layers and the poor thermal reflection performance of the prepared coating, which need to be solved urgently.

[0004] The use of a multi-phase, multi-layer coating structure can better solve this problem, but when conventional APS sprays multiple layers of alternating coatings, it is difficult to solve the problem of uniformity between the layers within the coating. Under working conditions with thickness restrictions and weight gain restrictions, conventional APS is difficult to achieve the preparation of multiple layers of alternating coatings. It is particularly urgent to achieve low-cost preparation of lightweight, multi-layer heterogeneous materials, and obtain a new type of thermal resistance coating with excellent thermal resistance and thermal insulation effects while ensuring low weight gain of heat-resistant structural parts. Summary of the invention

[0005] The first aspect of the present invention aims to provide an atmospheric plasma spraying method to solve the technical problem that the overall thickness of the existing thermal barrier coating is too large.

[0006] The atmospheric plasma spraying method provided in the first aspect of the present invention includes an alternating layer thickness control step, in which a first parameter of a feeding device, a second parameter of a motion control device, a third parameter of a spraying system and feedback information of a thickness feedback system are obtained, and the feeding device, the motion control device and the spraying system are controlled.

[0007] The beneficial effects brought by the atmospheric plasma spraying method of the present invention are:

[0008] By acquiring the first parameter of the feeding device, the second parameter of the motion control device and the third parameter of the spraying system, as well as the feedback information of the thickness feedback system, the feeding device, the motion control device and the spraying system are controlled to work together to adjust the thickness of each layer of material sprayed, which is beneficial to reducing the overall thickness of the alternating multi-layer ceramic thermal insulation layer, so that the overall thickness and weight requirements of the coating can be met while ensuring the thermal insulation performance.

[0009] In an optional technical solution, the feeding device includes a turntable and a turntable speed control device, the turntable speed control device is electrically connected to the turntable, and the turntable speed control device controls the uniform powder feeding amount of the feeding device to reach 3g / min to 10g / min;

[0010] and / or,

[0011] The motion control device is used to control the movement of a manipulator or other mobile platform for driving the plasma spray gun to move horizontally. The motion control device controls the horizontal movement speed of the plasma spray gun to reach 500mm / s to 2000mm / s.

[0012] In an optional technical solution, the thickness feedback accuracy of the thickness feedback system is less than 1 μm.

[0013] In an optional technical solution, the thickness feedback system obtains the coating thickness by at least one of metallographic thickness measurement, thickness gauge thickness measurement, blue light scanning and three-coordinate measuring instrument measurement.

[0014] In an optional technical solution, the spray control system includes controlling the parameters of the plasma spraying. In the plasma spraying, the spraying distance is 70mm~130mm, the spraying power is 15kw~80kw, the delivery gas flow rate is 6L / min~7L / min, the spraying angle is 75°~90°, the preheating temperature is 250℃~350℃, and the powder delivery pressure is 0.15MPa~0.3MPa.

[0015] The optional technical solution also includes: controlling the parameters of the pre-treatment step, in which 100# to 120# white corundum is used for sandblasting.

[0016] The second aspect of the present invention aims to provide a thermal barrier coating to solve the technical problem that the overall thickness of the thermal barrier coating is too large.

[0017] The thermal barrier coating provided in the second aspect of the present invention is prepared by any of the above-mentioned atmospheric plasma spraying methods; the thermal barrier coating includes a metal bonding layer and an alternating multilayer ceramic insulation layer, and the metal bonding layer and the alternating multilayer ceramic insulation layer are arranged in sequence from the substrate.

[0018] By arranging the above-mentioned atmospheric plasma spraying method in the thermal barrier coating, accordingly, the thermal barrier coating has all the advantages of the above-mentioned atmospheric plasma spraying method, which will not be described one by one here.

[0019] In an optional technical solution, the thermal barrier coating further comprises a surface low infrared emissivity coating disposed on the surface of the alternating multilayer ceramic insulation layer, and the surface low infrared emissivity coating is selected from precious metals or high temperature dielectric ceramic materials.

[0020] In an optional technical solution, the alternating multilayer ceramic thermal insulation coating uses at least two different high-temperature thermal barrier materials, the high-temperature thermal barrier materials include YSZ, GZO, Al2O3, rare earth zirconates, and cerates. The sprayed high-temperature thermal barrier material should be spherical powder or nearly spherical powder, and the particle size of the spherical powder and the nearly spherical powder is between 15μm and 70μm.

[0021] In an optional technical solution, the number of materials of the alternating multilayer ceramic thermal insulation coating is 2 to 20 layers; and the average thickness of each layer is 5 μm to 50 μm.

[0022] By arranging the above-mentioned atmospheric plasma spraying method in the thermal barrier coating, accordingly, the thermal barrier coating has all the advantages of the above-mentioned atmospheric plasma spraying method, which will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the background technology, the drawings required for use in the embodiments or the background technology description will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0024] Figure 1 A schematic diagram of a process flow of an atmospheric plasma spraying method provided by an embodiment of the present invention;

[0025] Figure 2 is a schematic diagram of a typical coating cross section in Example 1 of the present invention;

[0026] Figure 3 is a schematic diagram of a typical coating cross section in Example 2 of the present invention;

[0027] Figure 4 is a schematic diagram of a typical coating cross section in Example 3 of the present invention;

[0028] Figure 5 It is a schematic diagram of a typical coating cross section in Example 4 of the present invention. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] The atmospheric plasma spraying method provided by an embodiment of the present invention includes an alternating layer thickness control step. In the alternating layer thickness control step, a first parameter of a feeding device, a second parameter of a motion control device, a third parameter of a spraying system and feedback information of a thickness feedback system are obtained, and the feeding device, the motion control device and the spraying system are controlled.

[0031] By acquiring the first parameter of the feeding device, the second parameter of the motion control device and the third parameter of the spraying system, as well as the feedback information of the thickness feedback system, the feeding device, the motion control device and the spraying system are controlled to work together to adjust the thickness of each layer of material sprayed, which is beneficial to reducing the overall thickness of the alternating multi-layer ceramic thermal insulation layer, so that the overall thickness and weight requirements of the coating can be met while ensuring the thermal insulation performance.

[0032] The atmospheric plasma spraying method can solve the problem that atmospheric plasma spraying is not suitable for devices with restrictions on coating thickness, and can solve the problem of thickness uniformity of each layer in a multi-layer coating while achieving wide-range thickness control of a single coating.

[0033] The first parameter, the second parameter and the third parameter are not absolutely limited to one parameter, and the three names are used respectively for discussion based on relevant parameters of different devices or systems. In addition, when controlling the corresponding system, the corresponding parameters of the corresponding system are obtained in this embodiment, and adjustments are made according to the obtained parameters to manufacture a coating with a suitable thickness.

[0034] Optionally, the feeding device includes a turntable and a turntable speed control device, the turntable speed control device is electrically connected to the turntable, and the turntable speed control device controls the uniform powder feeding amount of the feeding device to reach 3g / min to 10g / min;

[0035] and / or,

[0036] The motion control device is used to control the movement of a manipulator or other mobile platform for driving the plasma spray gun to move horizontally. The motion control device controls the horizontal movement speed of the plasma spray gun to reach 500mm / s to 2000mm / s.

[0037] By controlling the uniform powder feeding amount and the moving speed of the plasma spray gun, the spraying efficiency can be effectively guaranteed to be moderate, and the spraying rate will not be too high, resulting in the inability to control the thickness in time.

[0038] Optionally, the thickness feedback system has a thickness accuracy of less than 1 μm.

[0039] The thickness feedback system with the above accuracy is selected to feedback the thickness, which can be applied to coatings with a thickness of only a few microns, which is beneficial to improve the thickness detection accuracy of the coating and ensure that the thickness of the coating meets the standard.

[0040] Optionally, the thickness feedback system obtains the coating thickness by at least one of metallographic thickness measurement, thickness gauge thickness measurement, blue light scanning and coordinate measuring machine measurement.

[0041] The above method is used to obtain the thickness of the coating, which not only meets the accuracy requirements, but also is easy to use online to quickly obtain thickness information and timely control the spraying of each coating to ensure the coating thickness.

[0042] Optionally, controlling the spraying system includes controlling parameters of plasma spraying. In plasma spraying, the spraying distance is 70mm~130mm, the spraying power is 15kw~80kw, the delivery gas flow rate is 6L / min~7L / min, the spraying angle is 75°~90°, the preheating temperature is 250℃~350℃, and the powder delivery pressure is 0.15MPa~0.3MPa.

[0043] Using the above parameters to control the operation of the spraying system can, on the one hand, improve the uniformity of the spraying thickness, and on the other hand, it is also conducive to ensuring that the spraying thickness is controllable.

[0044] Optionally, the method further comprises: controlling parameters of a pre-treatment step, wherein in the pre-treatment step, sandblasting is performed using 100# to 120# white corundum.

[0045] The use of white corundum of the above size for sandblasting is beneficial to clear the oxides on the surface of the substrate while properly ensuring the roughness of the substrate surface.

[0046] The thermal barrier coating provided in an embodiment of the present invention is prepared by any of the above-mentioned atmospheric plasma spraying methods; the thermal barrier coating includes a metal bonding layer and an alternating multilayer ceramic insulation layer, and the metal bonding layer and the alternating multilayer ceramic insulation layer are arranged in sequence from the substrate.

[0047] By arranging the above-mentioned atmospheric plasma spraying method in the thermal barrier coating, accordingly, the thermal barrier coating has all the advantages of the above-mentioned atmospheric plasma spraying method, which will not be described one by one here.

[0048] Optionally, the thermal barrier coating further comprises a surface low infrared emissivity coating disposed on the surface of the alternating multilayer ceramic insulation layer, the surface low infrared emissivity coating being selected from a noble metal or a high temperature dielectric ceramic material. The infrared emissivity of the surface low infrared emissivity coating is lower than 0.2 in the waveband of 2 microns to 20 microns.

[0049] By setting a low infrared emissivity coating on the surface, on the basis of thermal insulation of alternating multi-layer ceramic thermal insulation coatings, the external infrared emissivity can also be reduced, which is beneficial to improving the infrared stealth capability of the material using the coating.

[0050] Specifically, in this embodiment, the precious metal can be Pt, Au or Ir.

[0051] Optionally, the alternating multilayer ceramic thermal insulation coating uses at least two different high-temperature thermal barrier materials, the high-temperature thermal barrier materials include YSZ, GZO, Al2O3, rare earth zirconates, and cerates. The sprayed high-temperature thermal barrier material should be spherical powder or nearly spherical powder, and the particle size of the spherical powder and the nearly spherical powder is between 15μm and 70μm.

[0052] By arranging alternating multiple layers of ceramic thermal insulation coatings using the above materials and using spherical powder or near-spherical powder for spraying, the powder can be effectively melted and evenly distributed on the surface of the previous layer of material during the spraying process, thereby achieving multi-layer uniform distribution of the thermal insulation coating.

[0053] The nearly spherical powder in this embodiment can be such that the dimensions of each powder in different directions are no less than 80% of the maximum dimension.

[0054] Optionally, the number of materials of the alternating multilayer ceramic thermal insulation coating is 2 to 20 layers; and the average thickness of each layer is 5 μm to 50 μm.

[0055] Setting the number of materials in the coating to the above number of layers is conducive to increasing the number of contacting surfaces of different layers, which can significantly reduce the speed of heat transfer in different media to achieve the function of thermal barrier. Moreover, by controlling the thickness to the above value, a thin and light heterogeneous material multi-layer alternating coating structure can be prepared, which ensures low weight gain of temperature-resistant structural parts while relying on multi-layer alternating heterogeneous materials and interface and surface low emissivity layers to obtain excellent thermal resistance and thermal insulation effects.

[0056] Figure 1 A schematic diagram of a process flow of an atmospheric plasma spraying method provided by an embodiment of the present invention; Figure 1 As shown above, in summary, the atmospheric plasma spraying method provided by the present invention comprises the following steps:

[0057] S1: pre-treat the substrate;

[0058] S2: preparing a metal bonding layer on the substrate;

[0059] S3: preparing an alternating multilayer ceramic thermal insulation layer on the metal bonding layer; specifically comprising:

[0060] The feeding device, motion control device and spraying system are controlled to operate with corresponding parameters to spray the coating. The thickness feedback system obtains feedback information. If the thickness of the layer does not meet the standard, the material of the layer continues to be sprayed. If the thickness of the layer meets the standard, it is determined whether the number of coatings meets the standard. If not, other ceramic insulation layers continue to be sprayed. If it meets the standard, S4 is executed.

[0061] S4: Selectively prepare a surface low infrared emissivity coating as needed.

[0062] S5: Obtaining a thermal barrier coating.

[0063] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the following four embodiments are given for detailed description. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0064] Embodiment 1:

[0065] Taking GH625 as the matrix, NiCrAlY powder and 8YSZ powder are selected as the spraying powder materials. The powder shape is spherical powder, and its particle size range is between 20μm and 45μm. Use a manipulator to set the parallel movement speed of the plasma spray gun along the workpiece to 1000mm / s, select 100# white corundum sandblasting for matrix pretreatment, select 70mm for spraying distance, spray power of 15KW, powder feeding gas flow rate of 6L / min, spraying angle of 90°, preheating temperature of 250℃, and powder feeding pressure of 0.2MPa. The powder tray is surface ground and polished, and the powder feeding amount of both powders is set to 5g / min. The thickness feedback is obtained using metallographic method, and the thickness is 7μm. The typical cross-sectional morphology of the coating obtained is shown in the attached figure. Figure 2 shown.

[0066] Embodiment 2:

[0067] Taking GH625 as the matrix, the spray powder materials are NiCrAlY powder, 8YSZ powder, and GZO powder. The powder shape is spherical powder, and its particle size range should be between 20μm and 45μm. Use a manipulator to move the plasma spray gun parallel to the workpiece at a speed of 750mm / s. APS pre-treatment selects 100# white corundum sandblasting, the spraying distance is 70mm, the spraying power is 30KW, the powder feeding gas flow is 6L / min, the spraying angle is 90°, the preheating temperature is 250℃, and the powder feeding pressure is 0.2MPa. Set the NiCrAlY powder feeding amount to 8g / min, the 8YSZ powder feeding amount to 6g / min, and the GZO powder feeding amount to 6g / min. According to the powder feeding order of NiCrAlY, YSZ, GZO, YSZ, and GZO, spray according to the above operations. The thickness feedback was obtained by metallographic method, and a four-layer alternating ceramic coating with a total thickness of 90μm and a single layer thickness of 20μm was obtained. The typical cross-sectional morphology of the obtained coating is shown in the attached figure. Figure 3 shown.

[0068] Embodiment 3:

[0069] Taking GH625 as the matrix, the spray powder materials are NiCrAlY powder, 8YSZ powder, and GZO powder. The powder shape is spherical powder, and its particle size range should be between 20μm and 45μm. The plasma spray gun is moved parallel to the workpiece at a speed of 1000mm / s using a manipulator. APS pre-treatment is selected for 100# white corundum sandblasting, the spraying distance is 70mm, the spraying power is 30KW, the powder feeding gas flow is 6L / min, the spraying angle is 90°, the preheating temperature is 250℃, and the powder feeding pressure is 0.3MPa. The powder feeding rate of NiCrAlY powder is set to 8g / min, the powder feeding rate of 8YSZ powder is set to 5g / min, and the powder feeding rate of GZO powder is set to 5g / min. The powder feeding order of NiCrAlY, YSZ, GZO, YSZ, and GZO is sprayed according to the above operation, and then a high heat reflective functional layer with low infrared emissivity is prepared on the surface of the ceramic layer, with a thickness of about 5μm. The thickness feedback is obtained by metallographic method, and finally a multilayer thermal resistance coating with a single-layer ceramic thickness of 10μm, a total thickness of 40μm, four layers of alternating ceramics, and a high heat reflective coating on the surface is obtained. The typical cross-sectional morphology of the obtained coating is shown in the attached figure. Figure 4 shown.

[0070] Embodiment 4:

[0071] Taking GH625 stainless steel as the substrate, the spray powder materials are NiCrAlY powder, LSC powder, and Al2O3 powder. The powder shape is approximately spherical, and its particle size ranges from 20μm to 70μm. Use a manipulator to move the plasma spray gun parallel to the workpiece at a speed of 500mm / s. APS pretreatment selects 60# white corundum sandblasting, the spraying distance is 80mm, the spraying power is 35KW, the powder feeding gas flow is 7L / min, the spraying angle is 90°, the preheating temperature is 300℃, and the powder feeding pressure is 0.2MPa. The powder tray is surface ground and polished, and the NiCrAlY coating is prepared using the conventional APS method. The thickness is about 80 microns. The powder feeding amount of LSC powder and Al2O3 powder is 10g / min. According to the powder feeding order of LSC and Al2O3 powder, spray according to the above operation, and repeat the spraying twice. The thickness feedback was obtained by metallographic method, and finally the total thickness was 50μm, and the thickness of the single ceramic layer was about 20μm. The typical cross-sectional morphology of the obtained coating is shown in the attached figure. Figure 5 shown.

[0072] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

[0073] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the term "comprises" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprises a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0074] In the above embodiments, the descriptions of directions such as “upper” and “lower” are all based on the drawings.

[0075] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0076] Thus, the present invention will not be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. An atmospheric plasma spraying method, characterized in that: The method comprises an alternating layer thickness control step, in which a first parameter of a feeding device, a second parameter of a motion control device, a third parameter of a spraying system and feedback information of a thickness feedback system are obtained, and the feeding device, the motion control device and the spraying system are controlled.

2. The atmospheric plasma spraying method according to claim 1, characterized in that: The feeding device comprises a turntable and a turntable speed control device, wherein the turntable speed control device is electrically connected to the turntable, and the turntable speed control device controls the uniform powder feeding amount of the feeding device to reach 3g / min to 10g / min; and / or, The motion control device is used to control the movement of a manipulator or other mobile platform for driving the plasma spray gun to move horizontally. The motion control device controls the horizontal movement speed of the plasma spray gun to reach 500mm / s to 2000mm / s.

3. The atmospheric plasma spraying method according to claim 1, characterized in that: The thickness feedback system has a thickness accuracy of less than 1 μm.

4. The atmospheric plasma spraying method according to claim 3, characterized in that: The thickness feedback system obtains the coating thickness by at least one method selected from the group consisting of metallographic thickness measurement, thickness gauge thickness measurement, blue light scanning, and three-coordinate measuring machine measurement.

5. The atmospheric plasma spraying method according to any one of claims 1 to 4, characterized in that: The control spraying system includes parameters for controlling the plasma spraying. In the plasma spraying, the spraying distance is 70mm-130mm, the spraying power is 15kw-80kw, the delivery gas flow rate is 6L / min-7L / min, the spraying angle is 75°-90°, the preheating temperature is 250°C-350°C, and the powder delivery pressure is 0.15MPa-0.3MPa.

6. The atmospheric plasma spraying method according to any one of claims 1 to 4, characterized in that: Also includes: The parameters of the pre-treatment step are controlled. In the pre-treatment step, 100# to 120# white corundum is used for sandblasting.

7. A thermal barrier coating, characterized in that: The thermal barrier coating is prepared by the atmospheric plasma spraying method according to any one of claims 1 to 6; the thermal barrier coating comprises a metal bonding layer and an alternating multilayer ceramic insulation layer, wherein the metal bonding layer and the alternating multilayer ceramic insulation layer are sequentially arranged from a substrate.

8. The thermal barrier coating according to claim 7, characterized in that: The thermal barrier coating further comprises a surface low infrared emissivity coating disposed on the surface of the alternating multilayer ceramic insulation layer, and the surface low infrared emissivity coating is selected from noble metals or high temperature dielectric ceramic materials.

9. The thermal barrier coating according to claim 7, characterized in that: The alternating multilayer ceramic thermal insulation coating uses at least two different high-temperature thermal barrier materials, which include YSZ, GZO, Al2O3, rare earth zirconate and cerate. The sprayed high-temperature thermal barrier material should be spherical powder or nearly spherical powder, and the particle size of the spherical powder and the nearly spherical powder is between 15μm and 70μm.

10. The thermal barrier coating according to claim 7, characterized in that: The number of materials of the alternating multilayer ceramic heat-insulating coating is 2 to 20 layers; the average thickness of each layer is 5 μm to 50 μm.

Citation Information

Patent Citations

  • Spraying system

    CN108504982A

  • Multi-axis linkage spraying device and spraying method for thermal barrier coating on surface of special-shaped structural member

    CN109590139A

  • Double-layer thermal barrier / high-temperature low-infrared emissivity integrated coating, metal composite material with coating and preparation method thereof

    CN110055486A

  • Novel thermal barrier coating with high heat-insulating property and preparation process of novel thermal barrier coating

    CN114059001A

  • Method for machining cooling hole of heavy-duty gas turbine combustion chamber component with thermal barrier coating

    CN116716569A