Moisture-absorbing breathable superfine fiber synthetic leather

Through the formation of modified sea-island fibers and composite fibers and treatment with chemical nucleating agents, a multi-dimensional network and broken chain structures are formed, which solves the problems of insufficient impact resistance and heat resistance in the existing technology, and improves the moisture-absorbing, breathable and ultra-fine The structural strength and heat resistance of fiber synthetic leather enable better service life and performance.

CN118756501AActive Publication Date: 2024-10-11FUJIAN ZHONGYU WATERBORNE MICROFIBER TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410900385.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-11
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

The existing moisture-absorbing and breathable microfiber polyurethane synthetic leather has deficiencies in impact resistance, oxidation resistance and heat resistance, making it difficult to meet high-standard application requirements.

Method used

Using modified sea-island fiber and composite fiber, it forms a multi-dimensional network structure and breakage through cloth forming, needle punching, shrinkage shaping, impregnation, fiber reduction and drying processes, combined with modified ethylene polymer and chemical nucleating agent treatment. Chain structure to improve structural strength and heat resistance.

Benefits of technology

It effectively improves the structural strength and heat resistance of moisture-absorbing and breathable microfiber synthetic leather, extends its service life, improves breathability and water absorption, and solves the problems of poor heat resistance, oxidation resistance and sunlight aging resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004930315410000071
    Figure BDA0004930315410000071
  • Figure BDA0004930315410000081
    Figure BDA0004930315410000081
Patent Text Reader

Abstract

The invention discloses moisture-absorbing breathable superfine fiber synthetic leather, and relates to the technical field of synthetic leather, the moisture-absorbing breathable superfine fiber synthetic leather is prepared from modified sea-island fibers and composite fibers through cloth forming, needling shrinkage shaping, impregnation, reduction splitting, drying and post-treatment; wherein the modified sea-island fiber is prepared from polyamide 6 and a modified ethylene polymer according to a mass ratio of (3-8): 11; the composite fiber is prepared by melting and spinning chain-extended PET and low-density polyethylene according to the mass ratio of (12-16): (3-7), wherein the chain-extended PET is obtained by treating PET with a chemical nucleating agent and then mixing the treated PET with dipropylene glycol dimethacrylate for chain extension repair; the modified ethylene polymer comprises polymer resin composed of ethylene with at least two modified groups and butylene, hexene or octene, and the modified groups are polyether groups, amino groups, hydroxyl groups, carboxyl groups, amide groups, aldehyde groups, carbonyl groups, sulfonic acid groups, acyl chloride groups or phosphate groups. The composite material has the effects of impact resistance, oxidation resistance, heat resistance and effective improvement of air permeability and water absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of synthetic leather, and in particular to a moisture-absorbing and breathable ultrafine fiber synthetic leather. Background Art

[0002] Natural leather resources are limited, and the development of excellent simulated synthetic leather has become a trend. At present, the world's microfiber synthetic leather production has exceeded 100 million square meters, but it is still in short supply. Although the production of non-microfiber artificial leather and synthetic leather is large, it is difficult to meet the high standards of human beings. With the continuous advancement and improvement of production and application technology, the gradual decline in production costs, the change of people's consumption concepts and the enhancement of environmental awareness, the production and consumption of microfiber synthetic leather has grown rapidly, and it has been widely used in high-end shoes, clothing, furniture, balls, and automotive interiors. According to statistics, more than 90% of the world's high-end sports shoes are made of microfiber synthetic leather.

[0003] The Chinese patent application document with publication number 201410754335.2 discloses a method for preparing a moisture-absorbing and breathable ultrafine fiber polyurethane synthetic leather, which comprises the following steps: (1) Preparation of ultrafine denier sea-island fibers and non-woven fabrics: using polyamide 6 and low-density polyethylene as raw materials to prepare ultrafine denier indefinite island-island staple fibers of equal length, opening and combing the prepared ultrafine denier indefinite island-island staple fibers into a web, and then repeatedly puncturing the fibers up and down with high acupuncture density to prepare a non-woven fabric; after being rolled, the fibers are heat-shrinked and shaped at a temperature of 90 to 140°C, a speed of 5 to 8 m / min, a non-woven fabric density of 0.3 to 0.35 g / m2, and a shaping roller gap of The ratio of the thickness of the non-woven fabric to the thickness of the non-woven fabric is 1.1 to 1.5, thereby obtaining an ironed non-woven fabric; (2) wet impregnation: the non-woven fabric obtained in step (1) is impregnated with a polycarbonate polyurethane impregnation liquid, the modulus of the impregnation liquid is 50 to 90 kg / cm2, and the solid content is 12 to 16%, and then the non-woven fabric is squeezed and impregnated with a roller, and the impregnation liquid on both sides of the non-woven fabric is scraped clean with a scraper, and then solidified and foamed with a dimethylformamide aqueous solution with a mass concentration of 15 to 25%, and then washed with water to remove the residual dimethylformamide on the non-woven fabric, thereby obtaining a porous elastomeric polycarbonate polyurethane non-woven fabric wet base; (3) toluene reduction and drying; (4) peeling treatment; (5) grinding and dust removal; (6) three-plate, dyeing, embossing, ironing and rubbing.

[0004] However, when the preparation method of the moisture-absorbing and breathable microfiber polyurethane synthetic leather uses polyamide 6 and low-density polyethylene as raw materials to prepare sea island staple fibers, the material properties have certain disadvantages in terms of impact resistance, oxidation resistance and heat resistance. Therefore, when applied to synthetic leather, there is a problem of insufficient strength and toughness, which needs to be improved. Summary of the invention

[0005] In view of this, the purpose of this application is to provide a moisture-absorbing and breathable ultrafine fiber synthetic leather to achieve the purpose of improving impact resistance, oxidation resistance, heat resistance, air permeability and water absorption. The specific scheme is as follows:

[0006] A moisture-absorbing and breathable ultrafine fiber synthetic leather, comprising modified sea-island fiber and composite fiber, and is obtained through cloth-making, needle-punching, shrinkage and shaping, impregnation, fiber-opening, drying and post-treatment; wherein:

[0007] The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 3-8:11;

[0008] The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to extend the chain to obtain extended PET and low-density polyethylene in a mass ratio of 12-16:3-7;

[0009] The modified ethylene polymer includes a polymer resin composed of ethylene and butene, hexene or octene with at least two modified groups, and the modified groups are polyether groups, amino groups, hydroxyl groups, carboxyl groups, amide groups, aldehyde groups, carbonyl groups, sulfonic acid groups, acyl chloride groups or phosphoric acid groups.

[0010] Preferably, the modified group accounts for 0.5-12wt% of the modified ethylene polymer, and the melt index of the modified ethylene polymer is 22-60g / 10min.

[0011] Preferably, the modified sea-island fibers and the composite fibers are respectively webbed into composite cloth or woven into cloth in a mass ratio of 6-10:15-25, and then shrunken and shaped by needle punching to obtain composite sea-island fiber cloth.

[0012] Preferably, the impregnation is to place the composite island fiber into a polyurethane solution for impregnation treatment, wherein the polyurethane solution has a solid content of 8.6-11.2% and a modulus of 30-85 kg / cm 2 After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

[0013] Preferably: the modified ethylene polymer also includes a polymer resin composed of ethylene with a modified group and butene, hexene or octene, and the modified group is a polyether group, an amino group, a hydroxyl group, a carboxyl group, an amide group, an aldehyde group, a carbonyl group, a sulfonic acid group, an acyl chloride group or a phosphoric acid group.

[0014] Preferably, the modified group accounts for 0.5-12wt% of the modified ethylene polymer, and the melt index of the modified ethylene polymer is 37-60g / 10min.

[0015] Preferably, the chemical nucleating agent is talc, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 80-90:9.99-15:0.01-5.

[0016] Preferably: in the modified sea-island fiber, the polyamide 6 is an island phase, and the modified ethylene polymer is a sea phase; the intrinsic viscosity of the PET is 0.80-0.82 dL / g.

[0017] It can be seen from the above scheme that the present application provides a moisture-absorbing and breathable microfiber synthetic leather, which has the following beneficial effects:

[0018] 1. By modifying the sea-island fiber and the composite fiber into cloth, the base step of the moisture-absorbing and breathable ultrafine fiber synthetic leather can effectively improve the structural strength, achieve the purpose of anti-oxidation and heat resistance during long-term use, effectively extend the service life, and have effective air permeability and water absorption during use;

[0019] 2. When preparing the modified sea-island fiber by reacting the polymer resin formed by ethylene with a modified group and butene, hexene or octene with polyamide 6, the polymer resin forms a multi-dimensional network structure during the molding process with polyamide 6, thereby avoiding the phenomenon of island merging or island loss, and effectively controlling the production cost of the modified sea-island fiber, solving the problem of poor heat resistance, oxidation resistance and sunlight aging resistance of polyethylene;

[0020] 3. Treating PET with a chemical nucleating agent to form a chain-breaking structure on PET, so that when mixed with dipropylene glycol dimethacrylate to form a chain extension reaction, the lipid group and ether bond in dipropylene glycol dimethacrylate are combined with PET to form a polymer grid structure for improving the structural strength of the moisture-absorbing and breathable microfiber synthetic leather;

[0021] 4. By combining a polymer resin composed of ethylene with one modified group and butene, hexene or octene and a polymer resin composed of ethylene with at least two modified groups and butene, hexene or octene, the structural strength of the modified sea-island fiber is further improved, and the breakage and cross-linking of the polymer chain are effectively inhibited, thereby achieving the effect of effectively improving the heat resistance, oxidation resistance and sunlight aging resistance;

[0022] 5. By reacting a chemical nucleating agent composed of talcum powder, zinc pyrrolidone carboxylate and zinc stearate with PET, a multi-segment broken chain structure is formed on PET, so that dipropylene glycol dimethacrylate can be introduced into PET through chain extension, thereby improving the material structural strength of PET and enabling the composite fiber to adsorb the modified sea-island fiber, thereby improving the overall structural stability of the moisture-absorbing and breathable ultrafine fiber synthetic leather. DETAILED DESCRIPTION

[0023] The following will be clearly and completely described in conjunction with the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0024] It should be mentioned that in the embodiment of the moisture-absorbing and breathable ultrafine fiber synthetic leather of the present application, the preparation process of the modified sea-island fiber adopts the existing sea-island preparation process, such as the conjugate composite spinning method or the blended spinning method, and the preparation process of the composite fiber prepared by melt spinning adopts the existing fiber preparation process, which will not be described in detail here. The post-treatment is oiling and surface rubbing processing to make the surface of the synthetic leather close to the leather structure, improving the aesthetics and touch effect.

[0025] The following is a detailed description of a moisture-absorbing and breathable microfiber synthetic leather of the present application.

[0026] A moisture-absorbing and breathable ultrafine fiber synthetic leather, comprising modified sea-island fiber and composite fiber, and is obtained through cloth-making, needle-punching, shrinkage and shaping, impregnation, fiber-opening, drying and post-treatment; wherein:

[0027] The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 3-8:11. Polyamide 6 is an island phase, the modified ethylene polymer is a sea phase, and the intrinsic viscosity of PET is 0.80-0.82 dL / g.

[0028] It should be mentioned that the modified ethylene polymer includes a polymer resin composed of ethylene and butene, hexene or octene with at least two modified groups, and the modified groups are polyether groups, amino groups, hydroxyl groups, carboxyl groups, amide groups, aldehyde groups, carbonyl groups, sulfonic acid groups, acyl chloride groups or phosphoric acid groups. In the polymer resin composed of ethylene and butene, hexene or octene containing at least two modified groups, the modified groups account for 0.5-12wt% of the modified ethylene polymer by mass, and the melt index of the modified ethylene polymer is 22-60g / 10min.

[0029] In order to further improve the structural strength and stability, the modified ethylene polymer in some embodiments of the present application also includes a polymer resin composed of ethylene with a modified group and butene, hexene or octene. In the polymer resin composed of ethylene with a modified group and butene, hexene or octene, the modified group accounts for 0.5-12wt% of the modified ethylene polymer by mass, and the melt index of the modified ethylene polymer is 37-60g / 10min.

[0030] The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to extend the chain to obtain extended PET and low-density polyethylene in a mass ratio of 12-16:3-7.

[0031] In the embodiment of the present application, the modified island fiber and the composite fiber are respectively formed into a composite cloth or woven into a cloth in a mass ratio of 6-10:15-25, and then the composite island fiber cloth is obtained by needle punching and shrinking. The impregnation is to arrange the composite island fiber into a polyurethane solution for impregnation treatment, and the solid content of the polyurethane solution is 8.6-11.2%, and the modulus is 30-85kg / cm 2 After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

[0032] In order to achieve effective chain breaking of PET to facilitate mixed chain extension of dipropylene glycol dimethacrylate, the chemical nucleating agent in the embodiment of the present application is talcum powder, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 80-90:9.99-15:0.01-5.

[0033] Embodiment 1

[0034] A moisture-absorbing and breathable ultrafine fiber synthetic leather, comprising modified sea-island fiber and composite fiber, and is obtained through cloth-making, needle-punching, shrinkage and shaping, impregnation, fiber-opening, drying and post-treatment; wherein:

[0035] The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 3:11. Polyamide 6 is the island phase, the modified ethylene polymer is the sea phase, and the intrinsic viscosity of PET is 0.80 dL / g.

[0036] It should be mentioned that the modified ethylene polymer includes a polymer resin composed of ethylene and octene with three modified groups, and in the polymer resin composed of ethylene and octene with three modified groups, the polymer resin contains 3wt% of carboxyl groups, 1wt% of hydroxyl groups and 1wt% of phosphate groups, and the melt index of the modified ethylene polymer is 39g / 10min.

[0037] The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to obtain chain-extending repaired extended PET and low-density polyethylene in a mass ratio of 12:3.

[0038] In the embodiment of the present application, the modified island fiber and the composite fiber are respectively formed into a composite cloth or woven into a cloth in a mass ratio of 6:15, and then the composite island fiber cloth is obtained by needle punching and shrinking. Impregnation is to arrange the composite island fiber into a polyurethane solution for impregnation treatment. The solid content of the polyurethane solution is 8.6%, and the modulus is 30kg / cm 2After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

[0039] In order to achieve effective chain breaking of PET to facilitate mixed chain extension of dipropylene glycol dimethacrylate, the chemical nucleating agent in the embodiment of the present application is talcum powder, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 80:15:5.

[0040] Embodiment 2

[0041] A moisture-absorbing and breathable ultrafine fiber synthetic leather, comprising modified sea-island fiber and composite fiber, formed into cloth, needle-punched to shrink and shape, impregnated, reduced and opened, dried and post-treated; wherein:

[0042] The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 5:11. Polyamide 6 is the island phase, the modified ethylene polymer is the sea phase, and the intrinsic viscosity of PET is 0.81 dL / g.

[0043] It should be mentioned that the modified ethylene polymer includes a polymer resin composed of ethylene and hexene with two modified groups, and in the polymer resin composed of ethylene and hexene with two modified groups, the polymer resin contains 3.5wt% of polyether groups and 2.5wt% of sulfonic acid groups, and the melt index of the modified ethylene polymer is 45g / 10min.

[0044] The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to obtain chain-extending repaired extended PET and low-density polyethylene in a mass ratio of 13:5.

[0045] In the embodiment of the present application, the modified island fiber and the composite fiber are respectively formed into a composite cloth or woven into a cloth in a mass ratio of 7:21, and then the composite island fiber cloth is obtained by needle punching and shrinking. Impregnation is to arrange the composite island fiber into a polyurethane solution for impregnation treatment. The solid content of the polyurethane solution is 9.6%, and the modulus is 44kg / cm 2 After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

[0046] In order to achieve effective chain breaking of PET to facilitate mixed chain extension of dipropylene glycol dimethacrylate, the chemical nucleating agent in the embodiment of the present application is talcum powder, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 85:13:2.

[0047] Embodiment 3

[0048] A moisture-absorbing and breathable ultrafine fiber synthetic leather, comprising modified sea-island fiber and composite fiber, formed into cloth, needle-punched to shrink and shape, impregnated, reduced and opened, dried and post-treated; wherein:

[0049] The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 8:11. Polyamide 6 is the island phase, the modified ethylene polymer is the sea phase, and the intrinsic viscosity of PET is 0.82 dL / g.

[0050] It should be mentioned that the modified ethylene polymer includes a polymer resin composed of ethylene and butene with two modified groups, and in the polymer resin composed of ethylene and butene with two modified groups, the polymer resin contains 0.5wt% of carbonyl group and 8wt% of amide group, and the melt index of the modified ethylene polymer is 43g / 10min.

[0051] The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to extend the chain to obtain extended PET and low-density polyethylene in a mass ratio of 16:3.

[0052] In the embodiment of the present application, the modified island fiber and the composite fiber are respectively formed into a composite cloth or woven into a cloth in a mass ratio of 6-10:15-25, and then the composite island fiber cloth is obtained by needle punching and shrinking. The impregnation is to arrange the composite island fiber into a polyurethane solution for impregnation treatment, and the solid content of the polyurethane solution is 11.2%, and the modulus is 85kg / cm 2 After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

[0053] In order to achieve effective chain breaking of PET to facilitate mixed chain extension of dipropylene glycol dimethacrylate, the chemical nucleating agent in the embodiment of the present application is talcum powder, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 90:9.99:0.01.

[0054] Embodiment 4

[0055] The difference between Example 4 and Example 1 is that the modified ethylene polymer in Example 4 also includes a polymer resin composed of ethylene with one modified group and octene. In the polymer resin composed of ethylene with one modified group and octene, the polymer resin contains 7wt% of carboxyl groups and 3wt% of acyl chloride groups, and the melt index of the modified ethylene polymer is 56g / 10min.

[0056] Embodiment 5

[0057] The difference between Example 5 and Example 2 is that the modified ethylene polymer in Example 5 also includes a polymer resin composed of ethylene and butene with one modified group, and the polymer resin composed of ethylene and butene with one modified group contains 1wt% of amino groups and 0.5wt% of sulfonic acid groups, and the melt index of the modified ethylene polymer is 47g / 10min.

[0058] Comparative Example 1

[0059] The difference between Comparative Example 1 and Example 2 is that in Comparative Example 1, ethylene polymer is used instead of modified ethylene polymer.

[0060] Comparative Example 2

[0061] The difference between Comparative Example 2 and Example 2 is that PET is used in Comparative Example 2 to replace the chain-extended PET.

[0062] Comparative Example 3

[0063] The difference between Comparative Example 3 and Example 2 is that the chemical nucleating agent used in Comparative Example 3 is sodium benzoate.

[0064] test:

[0065] 1. Test the tensile load and elongation at break according to GB / T 8949-2008;

[0066] 2. Carry out water absorption test according to GB / T 4689.21-2008;

[0067] 3. Carry out air permeability test according to QB / T 2799-2006;

[0068] 4. The test results are shown in Table 1 below.

[0069] Table 1 Performance test results of Examples 1 to 5 and Comparative Examples 1 to 3

[0070]

[0071]

[0072] It can be seen from Table 1 above that based on Example 1 and Example 4, in the modified ethylene polymer composed of a polymer resin composed of ethylene and octene with one modified group and a polymer resin composed of ethylene and octene with three modified groups, the prepared hygroscopic and breathable ultrafine fiber synthetic leather has better water absorption and is improved in structural strength to a certain extent; based on Example 2 and Comparative Example 1, Comparative Example 2 and Comparative Example 3, when modified ethylene polymer, extended chain PET and sodium benzoate are used, the water absorption of the obtained hygroscopic and breathable ultrafine fiber synthetic leather is improved to a certain extent, and the structural strength of the hygroscopic and breathable ultrafine fiber synthetic leather is improved through a multi-dimensional mesh result, so that the hygroscopic and breathable ultrafine fiber synthetic leather has the effect of improving impact resistance, oxidation resistance, heat resistance, and air permeability and water absorption.

[0073] In summary, the present application provides a hygroscopic and breathable microfiber synthetic leather. The hygroscopic and breathable microfiber synthetic leather is made by modifying the sea island fiber and the composite fiber to form a cloth, so that the base step of the obtained hygroscopic and breathable microfiber synthetic leather has the effect of effectively improving the structural strength, achieving the purpose of anti-oxidation and heat resistance during long-term use, effectively extending the service life, and having effective air permeability and water absorption during use. Among them, in terms of modified ethylene polymers, when a polymer resin formed by ethylene with a modified group and butene, hexene or octene is prepared with polyamide 6 to obtain modified sea island fibers, the polymer resin forms a multi-dimensional network structure during the molding process with polyamide 6, thereby avoiding the phenomenon of island merging or island loss, and effectively controlling the production and manufacturing cost of the modified sea island fibers, and solving the problems of poor heat resistance, oxidation resistance and sunlight aging resistance of polyethylene; at the same time, by combining a polymer resin composed of ethylene with one modified group and butene, hexene or octene and a polymer resin composed of ethylene with at least two modified groups and butene, hexene or octene, the structural strength of the modified sea island fibers will be further improved, and the effect of effectively improving the heat resistance, oxidation resistance and sunlight aging resistance will be achieved. In terms of chain extension PET and its chemical nucleating agent, PET is treated with a chemical nucleating agent to form a broken chain structure on PET for providing exchange groups, so that when it is mixed with dipropylene glycol dimethacrylate to form a chain extension reaction, the lipid group and ether bond in the dipropylene glycol dimethacrylate are combined with PET to form a polymer grid structure for improving the structural strength of the moisture-absorbing and breathable ultrafine fiber synthetic leather, so that a chemical nucleating agent composed of talcum powder, zinc pyrrolidone carboxylic acid and zinc stearate reacts with PET to form a multi-segment broken chain structure on PET, so that dipropylene glycol dimethacrylate can be introduced into PET through chain extension, thereby improving the material structural strength of PET, and making the composite fiber have adsorbed modified sea island fibers, thereby improving the overall structural stability of the moisture-absorbing and breathable ultrafine fiber synthetic leather.

[0074] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.

[0075] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0076] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A moisture-absorbing and breathable microfiber synthetic leather, characterized in that: The method comprises adopting modified sea island fiber and composite fiber, forming cloth, shrinking and shaping by needle punching, impregnation, fiber opening by weight reduction, drying and post-treatment; wherein: The modified sea-island fiber is prepared from polyamide 6 and modified ethylene polymer in a mass ratio of 3-8:11; The composite fiber is prepared by melt spinning PET treated with a chemical nucleating agent and then mixed with dipropylene glycol dimethacrylate to extend the chain to obtain extended PET and low-density polyethylene in a mass ratio of 12-16:3-7; The modified ethylene polymer includes a polymer resin composed of ethylene and butene, hexene or octene with at least two modified groups, and the modified groups are polyether groups, amino groups, hydroxyl groups, carboxyl groups, amide groups, aldehyde groups, carbonyl groups, sulfonic acid groups, acyl chloride groups or phosphoric acid groups.

2. The moisture-absorbing and breathable microfiber synthetic leather according to claim 1, characterized in that: The modified group accounts for 0.5-12wt% of the modified ethylene polymer, and the melt index of the modified ethylene polymer is 22-60g / 10min.

3. The moisture-absorbing and breathable microfiber synthetic leather according to claim 1, characterized in that: The modified sea-island fiber and the composite fiber are respectively meshed into a composite cloth or woven into a cloth in a mass ratio of 6-10:15-25, and then the composite sea-island fiber cloth is obtained by shrinking and shaping through needle punching.

4. The moisture-absorbing and breathable microfiber synthetic leather according to claim 3, characterized in that: The impregnation is to arrange the composite sea-island fiber into a polyurethane solution for impregnation treatment, and the polyurethane solution has a solid content of 8.6-11.2% and a modulus of 30-85 kg / cm 2 After the treatment of the padder, the synthetic leather blank to be reduced is obtained after the drying and curing treatment.

5. The moisture-absorbing and breathable microfiber synthetic leather according to claim 1, characterized in that: The modified ethylene polymer also includes a polymer resin composed of ethylene with a modified group and butene, hexene or octene, and the modified group is a polyether group, an amino group, a hydroxyl group, a carboxyl group, an amide group, an aldehyde group, a carbonyl group, a sulfonic acid group, an acyl chloride group or a phosphoric acid group.

6. The moisture-absorbing and breathable microfiber synthetic leather according to claim 5, characterized in that: The modified group accounts for 0.5-12wt% of the modified ethylene polymer, and the melt index of the modified ethylene polymer is 37-60g / 10min.

7. The moisture-absorbing and breathable microfiber synthetic leather according to claim 1, characterized in that: The chemical nucleating agent is talcum powder, zinc pyrrolidone carboxylate and zinc stearate in a mass ratio of 80-90:9.99-15:0.01-5.

8. The moisture-absorbing and breathable microfiber synthetic leather according to claim 1, characterized in that: In the modified sea-island fiber, the polyamide 6 is an island phase, and the modified ethylene polymer is a sea phase; the intrinsic viscosity of the PET is 0.80-0.82 dL / g.

Citation Information

Patent Citations

  • Preparation method of moisture-absorbing ventilating superfine fiber polyurethane synthetic leather

    CN104452326A

  • Dyeable polyolefin fiber and fibrous structure comprising same

    CN108779583A

  • Eco-friendly artificial leather for interior of automobile and manufacturing method thereof

    CN108948313A

  • Preparation method of full-aqueous dry pasted microfiber leather

    CN111101385A

  • Preparation method of high-moisture-absorption breathable lining leather

    CN116815417A