Method for solving cracking caused by thermal expansion and cold contraction by paving road with waste tire particles

By extracting rubber oil, steel wire and fiber from waste tire particles and mixing them with asphalt for road paving, the crack problem caused by thermal expansion and contraction of the old cement pavement is solved, the crack resistance and deformation resistance of the road are improved, and the service life is extended. lifespan and reduced environmental pollution, achieving a combination of economic and environmental benefits.

CN118756547APending Publication Date: 2024-10-11HUNAN YOUGUAN SPORTS MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140366.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Old cement concrete pavements are prone to cracks under changes in temperature and humidity and vehicle loads, leading to pavement cracking, shortening service life and increasing maintenance costs, affecting traffic safety and comfort.

Method used

Rubber oil, steel wire and fiber are extracted from waste tire particles and mixed with asphalt, stone and antioxidants. Road paving is carried out through a specific process to enhance the road's resistance to cracking and deformation.

Benefits of technology

Significantly improve the road's resistance to cracking and deformation, extend its service life, reduce maintenance costs, reduce traffic congestion and accident rates, reduce environmental pollution and disposal costs of waste tires, and achieve the integration of environmental protection and economic benefits .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756547A_ABST
    Figure CN118756547A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of road paving, in particular to a method for solving cracking caused by thermal expansion and cold contraction by paving a road with waste tire particles. The method comprises the following steps: 1, preparing raw materials; the method for solving cracking caused by thermal expansion and cold contraction by using the waste tire particles to pave the road comprises the following steps: step 1, preparing materials, step 2, extracting the waste tire particles, step 3, pretreating asphalt, step 4, mixing the materials, step 5, paving the road, and step 6, maintaining. The anti-cracking and anti-deformation performance of a road is greatly enhanced by adding the antioxidant, the asphalt performance, the strength, the toughness, the anti-cracking performance, the bearing capacity and the overall performance of the road paving material are improved, the service life is prolonged, the maintenance cost of the road is reduced, the traffic jam and the accident rate caused by road surface damage are reduced, and the service life of the road paving material is prolonged. Therefore, the comfort and the safety of vehicle driving are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road paving, in particular to a method for solving thermal expansion and contraction cracking by paving roads with waste tire particles. Background Art

[0002] In the field of road construction, asphalt is often added to cement pavement. This approach cleverly combines the advantages of cement pavement and asphalt pavement. With its excellent strength and stability, cement pavement lays a solid foundation for roads. However, cement pavement also has obvious shortcomings. It is not comfortable to drive, it is noisy during driving, and it is very sensitive to temperature changes and is prone to cracks.

[0003] Of particular concern is that the joints and cracks in the old cement concrete pavement itself will cause vertical and horizontal displacement. Under the multiple effects of stress caused by temperature and humidity changes and vehicle loads, these cracks continue to expand upwards and are eventually exposed on the surface of the overlay layer, causing the pavement to crack and rainwater to seep down. This situation greatly impairs the overall performance of the pavement and shortens its service life. Not only that, the subsequent maintenance costs have increased significantly, causing economic losses, but also causing many adverse effects on traffic safety and traffic efficiency, thereby affecting the comfort and safety of vehicle driving.

[0004] In view of this, a new method for paving roads that uses waste tire particles to solve the problem of thermal expansion and contraction cracking is urgently needed to improve the shortcomings of the existing technology. Summary of the invention

[0005] The purpose of the present invention is to provide a method for solving the problem of thermal expansion and contraction cracking when paving roads with waste tire particles, so as to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides a method for paving roads with waste tire particles to solve the problem of thermal expansion and contraction cracking, comprising the following steps:

[0007] S1.1. Raw material preparation: waste tire particles, asphalt, stone and antioxidants;

[0008] S1.2, Waste tire particle extraction: Rubber oil, steel wire and fiber are extracted from waste tire particles;

[0009] S1.3, asphalt pretreatment: heat the asphalt to 180-200℃;

[0010] S1.4, Mixing materials: Add rubber oil, steel wire, fiber, stone and antioxidant into the heated asphalt, stir and mix, and the stirring time is 40-60 minutes;

[0011] S1.5, Road paving: First, clean and level the road base; then use a paver to evenly spread the mixed materials on the base; then, use a roller to compact the paved road surface;

[0012] S1.6, Maintenance: Cover the road surface with moisturizing materials and maintain for 10-16 days. During the maintenance period, vehicles and pedestrians are prohibited from passing;

[0013] S1.7. Quality inspection: After the maintenance period, the road will be inspected for quality.

[0014] As a further improvement of the technical solution, in S1.2, the technology for extracting rubber oil from waste tire particles comprises the following steps:

[0015] S2.1. Crushing and screening: Use special crushing equipment to further crush the waste tire particles into fine particles, and then use screening equipment to screen the fine particles to obtain fine particles that meet the requirements;

[0016] S2.2, pyrolysis: the fine particles are placed in a pyrolysis furnace, and the fine particles are heated to 600-1000°C in an oxygen-deficient environment. During the pyrolysis process, the rubber is decomposed into at least gas, oil and solid carbon black;

[0017] S2.3, Condensation and separation: The gas produced by pyrolysis is cooled by a condensation device to form liquid oil, and the oil and solid carbon black are separated by physical methods;

[0018] S2.4, Refining: The separated rubber oil is refined to obtain high-quality rubber oil.

[0019] As a further improvement of the technical solution, in S1.2, the technology for extracting steel wire from waste tire particles includes the following steps:

[0020] S3.1. Crushing and grinding: further crushing and grinding of waste tire particles;

[0021] S3.2, Magnetic Separation: Use magnetic separation equipment to initially separate magnetic materials, including steel wire;

[0022] S3.3, wind separation and impurity removal: remove some lighter impurities and rubber debris through wind power;

[0023] S3.4, Vibration screening: Use a vibrating screen to further screen the particles according to their size and shape, so that the steel wire can be separated from other particles more thoroughly;

[0024] S3.5, pickling treatment: pickling the steel wire-containing materials obtained from the preliminary screening;

[0025] S3.6, Fine magnetic separation: Use high gradient magnetic separator to carry out fine magnetic separation of steel wire materials;

[0026] S3.7, Drying and Cooling: The separated steel wire is dried, and then naturally cooled in a room temperature environment to obtain high-purity steel wire.

[0027] As a further improvement of the technical solution, in S1.2, the fiber extraction technology of waste tire particles includes the following steps:

[0028] S4.1. Preliminary screening and soaking: Preliminary screening of waste tire particles, then soaking the screened waste tire particles in a specific chemical solution, which can soften the rubber and make the fibers easier to separate;

[0029] S4.2, mechanical stirring: mechanically stirring the mixture after soaking;

[0030] S4.3, Screening and separation: Use screening equipment to separate the fibers;

[0031] S4.4, cleaning and drying: The separated fibers are cleaned and then dried to obtain high-quality fibers.

[0032] As a further improvement of the technical solution, in S1.4, the amount of the rubber oil is 6%-16%, the amount of the steel wire is 2%-6%, the amount of the fiber is 0.2%-0.6%, the amount of the stone is 60%-75%, the amount of the antioxidant is 0.2%-0.6%, and the amount of asphalt is the remainder.

[0033] As a further improvement of the present technical solution, in S1.6, the moisturizing material is at least one of a plastic film and a geotextile, and the moisturizing material is preferably a plastic film.

[0034] As a further improvement of the present technical solution, in S4.1, the chemical solution adopts at least one of a surfactant solution, an organic solvent, and an alkaline solution, and the chemical solution preferably adopts an alkaline solution.

[0035] As a further improvement of the technical solution, the amount of the rubber oil is 16%, the amount of the steel wire is 5%, the amount of the fiber is 0.6%, the amount of the stone is 60%, the amount of the antioxidant is 0.4%, and the amount of asphalt is the balance.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1. In the method of using waste tire particles to pave roads to solve the problem of thermal expansion and contraction cracking, rubber oil, steel wire and fiber carefully extracted from waste tires are incorporated into the configuration of road paving materials, and antioxidants are added, which greatly enhances the road's resistance to cracking and deformation, improves the asphalt performance, strength, toughness, crack resistance, bearing capacity and overall performance of road paving materials, extends the service life, reduces road maintenance costs, reduces traffic congestion and accident rates caused by road damage, and thus improves the comfort and safety of vehicle driving.

[0038] 2. In the method of using waste tire particles to pave roads to solve the problem of thermal expansion and contraction cracking, the use of waste tire particles can not only solve the problem of thermal expansion and contraction cracking for paving roads, but also effectively alleviate the heavy pressure on the environment and reduce the space occupied by waste. At the same time, the accumulation of waste tires is greatly reduced, thereby effectively reducing the energy consumption in the process of waste tire processing, thereby improving the utilization rate and reducing costs.

[0039] 3. The method of using waste tire particles to pave roads to solve the problem of thermal expansion and contraction cracking not only effectively curbs the pollution and damage to the ecological environment caused by waste tires, but also cleverly uses recycling to significantly reduce the procurement cost of raw materials in the road construction process, thereby achieving a seamless integration of environmental and economic benefits. It not only reduces greenhouse gas emissions in the process of waste tire treatment, but also promotes the green transformation of related industries. At the same time, it creates new profit growth points for road construction companies, thereby promoting the sustainable development and virtuous cycle of the industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a flowchart of the road paving process of the present invention;

[0041] Figure 2 This is a flowchart of the process of extracting rubber oil from waste tire particles of the present invention;

[0042] Figure 3 This is a flowchart of the process of extracting steel wire from waste tire particles of the present invention;

[0043] Figure 4 This is a flowchart of the process of extracting fibers from waste tire particles of the present invention;

[0044] Figure 5 It is a schematic diagram of the detection indicators of each sample of the present invention. DETAILED DESCRIPTION

[0045] The following will be combined with the accompanying drawings in the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0046] according to Figure 1 As shown, the embodiment of the present invention also provides a method for preparing the above-mentioned method of using waste tire particles to pave roads to solve the problem of thermal expansion and contraction cracking, and the specific steps are as follows:

[0047] Step 1: Raw material preparation: Collect a large amount of waste tires and use professional crushing equipment to crush the tires into particles to obtain waste tire particles. Select asphalt materials that meet road construction standards, and then select wear-resistant and hard stones and antioxidants that can prevent waste tire particles from oxidizing and deteriorating at high temperatures;

[0048] Step 2: Extraction of waste tire particles: Extracting rubber oil, steel wire and fiber from waste tire particles;

[0049] Step 3: Asphalt pretreatment: Heat the asphalt to 180-200°C to make it have good fluidity;

[0050] Step 4. Mixing materials: Add 6%-16% rubber oil, 2%-6% steel wire, 0.2%-0.6% fiber, 60%-75% stone and 0.2%-0.6% antioxidant to the heated asphalt, stir and mix, and the stirring time is 40-60 minutes to ensure that all materials are evenly distributed.

[0051] Step 5: Road paving: First, clean and level the road base to ensure that the base is solid and flat; then use a paver to evenly spread the mixed materials on the base, and control the paving thickness and slope; then, use a roller to compact the paved road surface. The number of rolling times and compaction degree should be based on the road design requirements. Generally, it is rolled 4-6 times to ensure the density and flatness of the road surface;

[0052] Step 6: Maintenance: The paved road needs to be maintained. The road surface is covered with a moisturizing material. The moisturizing material is at least one of plastic film and geotextile. Plastic film is preferred for moisturizing material. The maintenance period is 10-16 days. During the maintenance period, vehicles and pedestrians are prohibited from passing to ensure that the road surface is fully solidified and stable during the maintenance process.

[0053] Step 7. Quality inspection: After the maintenance period, the road will be inspected for quality, including flatness, compaction and crack resistance, to ensure that the road quality meets the design requirements.

[0054] In order to further realize resource recycling, improve road performance and reduce the pressure of waste tires on the environment, therefore, in step three, the technology for extracting rubber oil from waste tire particles includes the following steps:

[0055] Step 1: Crushing and screening: Use special crushing equipment, preferably a crusher, or a grinder, to further crush the waste tire particles into fine particles, and then use screening equipment to screen the fine particles to obtain fine particles that meet the requirements;

[0056] Step 2, pyrolysis: the fine particles are placed in a pyrolysis furnace, and the fine particles are heated to 600-1000°C in an oxygen-deficient environment or in an inert gas environment. During the pyrolysis process, the rubber is decomposed into at least gas, oil and solid carbon black;

[0057] Step 3, condensation and separation: The gas generated by pyrolysis is cooled by a condensation device to form liquid oil, and the oil and solid carbon black are separated by physical methods, wherein: the physical method preferably adopts a centrifugal separation method, in which the pyrolysis product is placed in a centrifuge, and the solid carbon black with a higher density is deposited on the bottom or inner wall of the centrifuge by centrifugal force, while the oil is in the upper layer, thereby achieving separation; a precipitation method can also be adopted, in which the pyrolysis product is placed in a container and allowed to naturally precipitate under the action of gravity. Due to the high density of carbon black, it will gradually settle to the bottom, and the upper layer is oil, which can then be extracted from the upper layer;

[0058] Step 4: Refining: The separated rubber oil is refined to obtain high-quality rubber oil. The refining process includes filtering, distillation, chemical treatment and other steps, which are beneficial to remove impurities and harmful substances and improve the quality and purity of the rubber oil.

[0059] The technology of extracting steel wire from waste tire particles includes the following steps:

[0060] Step 1: Crushing and grinding: further crushing and grinding the waste tire particles to make them smaller in size for subsequent separation;

[0061] Step 2: Magnetic separation: Use magnetic separation equipment to initially separate magnetic substances, including steel wire;

[0062] Step 3: Wind separation and impurity removal: remove some lighter impurities and rubber debris through wind power;

[0063] Step 4: Vibration screening: Use a vibrating screen to further screen the particles according to their size and shape, so that the steel wire can be separated from other particles more thoroughly;

[0064] Step 5: Pickling: Pickle the steel wire material obtained in the preliminary selection to remove rust and impurities on the surface;

[0065] Step 6: Fine magnetic separation: Use a high gradient magnetic separator to perform fine magnetic separation on the steel wire material. The high gradient magnetic separator can produce a stronger magnetic field gradient and has a better separation effect on weakly magnetic materials, ensuring the purity of the steel wire;

[0066] Step 7, drying and cooling: Dry the separated steel wires, and then naturally cool the dried steel wires in a room temperature environment to avoid stress in the steel wires caused by rapid cooling, so as to obtain high-purity steel wires.

[0067] The technology for extracting fiber from waste tire particles includes the following steps:

[0068] Step 1: Preliminary screening and soaking: Preliminary screening of waste tire particles to remove oversized or undersized particles and other impurities, and then soak the screened waste tire particles in a specific chemical solution. The chemical solution uses at least one of a surfactant solution, an organic solvent, and an alkaline solution. The chemical solution preferably uses an alkaline solution, which can soften the rubber and make the fibers easier to separate;

[0069] Step 2: Mechanical stirring: Mechanically stirring the soaked mixture can accelerate the separation of rubber and fiber;

[0070] Step 3: Screening and separation: Use screening equipment to separate the fibers from other substances based on their size differences;

[0071] Step 4: Cleaning and drying: Clean the separated fibers to remove residual chemicals and impurities, and then dry the cleaned fibers to remove moisture to obtain high-quality fibers.

[0072] In the present invention, rubber oil, steel wire and fiber carefully extracted from waste tires are firstly added, and mixed with asphalt and stone to obtain road paving materials. The addition of rubber oil can improve the performance of asphalt, improve its elasticity and anti-aging performance, and the steel wire and fiber can increase the strength and toughness of the mixture, thereby enhancing the crack resistance and deformation resistance of the road. At the same time, the addition of antioxidants can also inhibit or delay the oxidation reaction of asphalt during use, reduce the oxidative degradation of waste tire particles during use, and extend its service life. The antioxidant may play a role in the following ways:

[0073] (1) Free radical capture: Antioxidants can react with free radicals and prevent them from initiating oxidative chain reactions.

[0074] (2) Hydrogen atom transfer: Antioxidants can provide hydrogen atoms to react with peroxides and interrupt the oxidation process.

[0075] (3) Metal ion chelation: Antioxidants can bind to metal ions and reduce their catalytic effect on oxidation reactions.

[0076] In the configuration of road paving materials, rubber oil, steel wire and fiber carefully extracted from waste tires are incorporated, and antioxidants are added, which greatly enhances the road's resistance to cracking and deformation, improves the asphalt performance, strength, toughness, crack resistance, bearing capacity and overall properties of road paving materials, extends its service life, reduces road maintenance costs, reduces traffic congestion and accident rates caused by road damage, and thus improves the comfort and safety of vehicle driving.

[0077] The use of waste tire particles not only solves the problem of thermal expansion and contraction cracking in road paving, but also effectively alleviates the heavy pressure on the environment and reduces the space occupied by waste. At the same time, the accumulation of waste tires is greatly reduced, thereby effectively reducing the energy consumption in the waste tire processing process, thereby increasing the utilization rate and reducing costs.

[0078] It not only effectively curbs the pollution and damage to the ecological environment caused by waste tires, but also cleverly uses recycling to significantly reduce the procurement cost of raw materials in the road construction process, thereby achieving a seamless integration of environmental benefits and economic benefits. It not only reduces greenhouse gas emissions in the process of waste tire treatment, but also promotes the green transformation of related industries. At the same time, it creates new profit growth points for road construction companies, thereby promoting the sustainable development and virtuous cycle of the industry.

[0079] According to different raw material dosages, the method for solving thermal expansion and contraction cracking in paving roads with waste tire particles provided by the present invention is further described through the following specific embodiments.

[0080] Example 1

[0081] The amount of rubber oil used is 6%, the amount of steel wire is 2%, the amount of fiber is 0.2%, the amount of stone is 75%, the amount of antioxidant is 0.2%, and the amount of asphalt is the balance.

[0082] First, heat the remaining asphalt to 180°C, then add 6% rubber oil, 2% steel wire, 0.2% fiber, 75% stone and 0.2% antioxidant to the heated asphalt and stir to mix. The stirring time is 45 minutes. After that, clean and level the road base. Use a paver to evenly spread the mixed materials on the base. Then, use a roller to compact the paved road surface and cover the road surface with moisturizing materials. Maintain for 10 days. During the maintenance period, vehicles and pedestrians are prohibited from passing. After the maintenance period, the road quality is inspected and the road paving is completed.

[0083] Example 2

[0084] The amount of rubber oil used is 16%, the amount of steel wire is 5%, the amount of fiber is 0.6%, the amount of stone is 60%, the amount of antioxidant is 0.4%, and the amount of asphalt is the balance.

[0085] First, heat the remaining asphalt to 200°C, then add 16% rubber oil, 5% steel wire, 0.6% fiber, 60% stone and 0.4% antioxidant to the heated asphalt and stir and mix for 60 minutes. After that, clean and level the road base first; then use a paver to evenly spread the mixed materials on the base; then use a roller to compact the paved road surface and cover the road surface with moisturizing materials for 14 days. During the maintenance period, vehicles and pedestrians are prohibited from passing. After the maintenance period, the road quality is inspected and the road paving is completed.

[0086] Example 3

[0087] The amount of rubber oil used is 12%, the amount of steel wire is 6%, the amount of fiber is 0.4%, the amount of stone is 70%, the amount of antioxidant is 0.6%, and the amount of asphalt is the balance.

[0088] First, heat the remaining asphalt to 190°C, then add 12% rubber oil, 6% steel wire, 0.4% fiber, 70% stone and 0.6% antioxidant to the heated asphalt and stir to mix for 50 minutes. After that, clean and level the road base. Use a paver to evenly spread the mixed materials on the base. Then, use a roller to compact the paved road surface and cover it with moisturizing materials for 16 days. During the maintenance period, vehicles and pedestrians are prohibited from passing. After the maintenance period, the road quality is inspected and the road paving is completed.

[0089] Table 1 Amount of each raw material used in Examples 1-3

[0090] Example 1 Example 2 Example 3 Rubber oil% 6 16 12 Steel wire % 2 5 6 fiber% 0.2 0.6 0.4 Stone % 75 60 70 Antioxidant % 0.2 0.4 0.6 Asphalt heating temperature℃ 180 200 190 Mixing time min 45 60 50 Maintenance 10 14 16

[0091] In order to verify that the paved road prepared in the embodiment of the present invention solves the thermal expansion and contraction cracking, the method for solving the thermal expansion and contraction cracking by paving the road with waste tire particles provided in the embodiment of the present invention is described through the following test group.

[0092] Experimental Group

[0093] The purpose of this test group is to explore the effects of different component ratios on solving thermal expansion and contraction cracking in paved roads.

[0094] Test objectives: To test the asphaltness, strength, toughness, crack resistance, load-bearing capacity and overall properties of the road paving material of the present invention.

[0095] Test method: Test group A, test group B and test group C respectively adopted the composition ratios of the road paving materials provided in Examples 1-3; the control example adopted control group A and control group B, wherein: control group A adopted the method of Example 2, but did not add rubber oil, steel wire and fiber, and did not add antioxidants, and control group B adopted the method of Example 1, but did not add antioxidants.

[0096] Specific detection indicators are shown in Table 2.

[0097] Table 2 Test indicators of each sample (points)

[0098] Test Group A Test Group B Test Group C Control group A Control group B Asphalt performance (points) 70 90 83 40 60 Strength (points) 65 85 80 50 65 Toughness (points) 60 80 75 40 55 Crack resistance (points) 60 90 80 40 55 Carrying capacity (points) 85 80 83 60 70 Overall performance (points) 70 88 80 45 60

[0099] according to Figure 5 As shown in Table 2, after adding rubber oil, steel wire, fiber and antioxidant, all performance indicators are significantly improved.

[0100] In terms of asphalt performance: the scores of the test groups A, B, and C were higher than those of the control groups A and B, indicating that the addition of these ingredients can significantly improve the asphalt performance; in terms of strength: the strength of the test groups was significantly higher than that of the control group, indicating that the addition of rubber oil, steel wire, and fiber enhanced the strength of the road; in terms of toughness: the toughness scores of the test groups were higher, better than those of the control group without these ingredients, reflecting the positive effect of additives on toughness; in terms of crack resistance: the crack resistance of the test groups was much better than that of the control group, highlighting the significant effect of component addition in resisting cracks; in terms of bearing capacity: the bearing capacity of the test groups was also generally better than that of the control group; in terms of overall performance: the test groups with the addition of key ingredients had higher overall performance scores.

[0101] The main reasons are: the addition of rubber oil, steel wire and fiber effectively improves the physical properties of road materials, such as strength, toughness and crack resistance, and the use of antioxidants helps to maintain the stability and durability of material properties.

[0102] Comprehensively considering various indicators, the performance of test group B (Example 2) is relatively outstanding. First, in terms of asphalt performance, its score is as high as 90 points, which is significantly better than the control group, which means that the road can maintain better performance under different temperature conditions and enhances the adaptability of the road; in terms of strength, the score of 85 points indicates that the road can withstand a larger load and reduce the risk of damage caused by heavy loads; the toughness performance of 80 points makes the road more elastic when facing external force impact and less prone to brittle failure; the crack resistance is as high as 90 points, which can effectively resist the cracks caused by temperature changes and vehicle driving, greatly extending the service life of the road; the bearing capacity is 80 points, which can adapt to larger traffic flows and heavier vehicles; the overall performance reaches 88 points, reflecting its balance and excellence in various performance indicators, which can provide strong guarantees for the safety, stability and long-term use of roads, reduce the frequency and cost of road maintenance and repair, thereby improving road quality while bringing significant economic and social benefits.

[0103] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for using waste tire particles to pave roads to solve the problem of thermal expansion and contraction cracking. It is characterized in that The following steps are involved: S1.

1. Raw material preparation: waste tire particles, asphalt, stone and antioxidants; S1.2, Waste tire particle extraction: Rubber oil, steel wire and fiber are extracted from waste tire particles; S1.3, asphalt pretreatment: heat the asphalt to 180-200℃; S1.4, Mixing materials: Add rubber oil, steel wire, fiber, stone and antioxidant into the heated asphalt, stir and mix, and the stirring time is 40-60 minutes; S1.5, Road paving: First, clean and level the road base; then use a paver to evenly spread the mixed materials on the base; then, use a roller to compact the paved road surface; S1.6, Maintenance: Cover the road surface with moisturizing materials and maintain for 10-16 days. During the maintenance period, vehicles and pedestrians are prohibited from passing; S1.

7. Quality inspection: After the maintenance period, the road will be inspected for quality.

2. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 1, Features: In S1.2, the technology for extracting rubber oil from waste tire particles includes the following steps: S2.

1. Crushing and screening: Use special crushing equipment to further crush the waste tire particles into fine particles, and then use screening equipment to screen the fine particles to obtain fine particles that meet the requirements; S2.2, pyrolysis: the fine particles are placed in a pyrolysis furnace, and the fine particles are heated to 600-1000°C in an oxygen-deficient environment. During the pyrolysis process, the rubber is decomposed into at least gas, oil and solid carbon black; S2.3, Condensation and separation: The gas produced by pyrolysis is cooled by a condensation device to form liquid oil, and the oil and solid carbon black are separated by physical methods; S2.4, Refining: The separated rubber oil is refined to obtain high-quality rubber oil.

3. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 1, Features: In S1.2, the technology for extracting steel wire from waste tire particles includes the following steps: S3.

1. Crushing and grinding: further crushing and grinding of waste tire particles; S3.2, Magnetic Separation: Use magnetic separation equipment to initially separate magnetic materials, including steel wire; S3.3, wind separation and impurity removal: remove some lighter impurities and rubber debris through wind power; S3.4, Vibration screening: Use a vibrating screen to further screen the particles according to their size and shape, so that the steel wire can be separated from other particles more thoroughly; S3.5, pickling treatment: pickling the steel wire-containing materials obtained from the preliminary screening; S3.6, Fine magnetic separation: Use high gradient magnetic separator to carry out fine magnetic separation of steel wire materials; S3.7, Drying and Cooling: The separated steel wire is dried, and then naturally cooled in a room temperature environment to obtain high-purity steel wire.

4. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 1, Features: In S1.2, the technology for extracting fibers from waste tire particles comprises the following steps: S4.

1. Preliminary screening and soaking: Preliminary screening of waste tire particles, then soaking the screened waste tire particles in a specific chemical solution, which can soften the rubber and make the fibers easier to separate; S4.2, mechanical stirring: mechanically stirring the mixture after soaking; S4.3, Screening and separation: Use screening equipment to separate the fibers; S4.4, cleaning and drying: The separated fibers are cleaned and then dried to obtain high-quality fibers.

5. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 1, Features: In S1.4, the amount of the rubber oil is 6%-16%, the amount of the steel wire is 2%-6%, the amount of the fiber is 0.2%-0.6%, the amount of the stone is 60%-75%, the amount of the antioxidant is 0.2%-0.6%, and the amount of asphalt is the balance.

6. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 1, Features: In S1.6, the moisturizing material is at least one of a plastic film and a geotextile, and the moisturizing material is preferably a plastic film.

7. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 4, Features: In S4.1, the chemical solution is at least one of a surfactant solution, an organic solvent, and an alkaline solution, and the chemical solution is preferably an alkaline solution.

8. The method for solving thermal expansion and contraction cracking when paving roads with waste tire particles according to claim 5, Features: The amount of the rubber oil is 16%, the amount of the steel wire is 5%, the amount of the fiber is 0.6%, the amount of the stone is 60%, the amount of the antioxidant is 0.4%, and the amount of the asphalt is the balance.