Method and system for researching collision of heterogeneous inclusions by using high-temperature confocal equipment

Studying the collision behavior of heterogeneous inclusions through high-temperature confocal equipment solves the problem of difficulty in observing and studying inclusion collisions in high-temperature molten steel with existing technology, and provides an in-depth understanding and practical application of inclusion removal rate and refining slag adsorption capacity. guide.

CN118758709APending Publication Date: 2024-10-11NORTH CHINA UNIVERSITY OF TECHNOLOGY +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410786537.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult to directly observe and study the collision behavior of heterogeneous inclusions in high-temperature molten steel with existing technology, which limits the in-depth understanding of inclusion removal rate and refining slag adsorption capacity.

Method used

High-temperature confocal equipment was used to conduct experiments. By preparing steel containing major inclusions and secondary inclusions, and conducting high-temperature confocal experiments in a non-vacuum state in a high-temperature confocal metallographic furnace, the collision behavior of heterogeneous inclusions was observed and recorded in real time. Analyze its ability to grow.

Benefits of technology

It achieves theoretical guidance on the collision trend of heterogeneous inclusions and its application in actual production. It improves the adsorption capacity of endogenous inclusions by adjusting the composition of the slag, and provides a more intuitive method for removing inclusions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118758709A_ABST
    Figure CN118758709A_ABST
Patent Text Reader

Abstract

The invention provides a method and a system for researching collision of heterogeneous inclusions by using high-temperature confocal equipment. The method comprises the following steps: preparing steel containing main inclusions and secondary inclusions by using the high-temperature equipment; the method comprises the following steps: placing steel containing main inclusions and secondary inclusions in a high-temperature confocal metallographic furnace, carrying out a high-temperature confocal experiment, observing the collision behavior of the foreign inclusions in real time, and recording and analyzing the positions of the inclusions at different moments to obtain the collision growth capability of the foreign inclusions. According to the method, the surface melting of the molten steel is better controlled by adopting new equipment (a high-temperature confocal microscope), and the adsorption capacity of the refining slag to the inclusions is more intuitively analyzed by simulating an actual steel slag environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method and a system for studying collision of heterogeneous inclusions by using a high-temperature confocal device. Background Art

[0002] Non-metallic inclusions in steel exist as independent phases. The composition, size, density and shape of inclusions in steel have an important influence on the mechanical properties and corrosion resistance of steel. The main behaviors of non-metallic inclusions in steel are: nucleation, growth, aggregation, growth and floating. Promoting the collision, aggregation, growth and floating of non-metallic inclusions is an important means to remove inclusions. It is not enough to remove inclusions by floating inclusions. Enhancing the collision between non-metallic inclusions to aggregate them into larger inclusions is an important means to improve the removal rate of non-metallic inclusions. At the same time, during the refining process, the refining slag will have a certain adsorption capacity for endogenous inclusions in steel, thereby achieving the adsorption of endogenous inclusions in steel.

[0003] During the refining process, the adsorption and collision abilities of refined slags of different compositions on the surface of molten steel and the internal inclusions of steel are different, and the collision and growth abilities of inclusions of different compositions in steel are also different. Therefore, it is of great research significance to explore the adsorption and collision abilities of heterogeneous inclusions. Because high-temperature molten steel is invisible, predecessors usually use numerical simulation and physical simulation methods to study the collision of heterogeneous inclusions. Few people directly observe the collision of heterogeneous inclusions through experimental means. A new experimental method is urgently needed to realize the observation of the collision behavior of heterogeneous inclusions. At present, high-temperature confocal microscope equipment is widely used in materials, metallurgy, welding and other fields. There are many studies on the mutual collision between internal inclusions in steel. Due to the limitations of experimental methods, it is difficult to study the collision behavior between heterogeneous inclusions. Now a method and system for studying the collision of heterogeneous inclusions using high-temperature confocal equipment is proposed. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method and system for studying the collision of heterogeneous inclusions using a high-temperature confocal device, which provides theoretical guidance for predicting the collision trend of inclusions. At the same time, the research results can be applied in the actual production process to achieve the adsorption of endogenous inclusions in steel by adjusting the composition of slag.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] The method for studying the collision of heterogeneous inclusions using a high temperature confocal device comprises the following steps:

[0007] Preparation of steel containing major inclusions and minor inclusions using high temperature equipment;

[0008] The steel containing major inclusions and minor inclusions were placed in a high-temperature confocal metallographic furnace for a high-temperature confocal experiment. The collision behavior of heterogeneous inclusions was observed in real time, and the positions of inclusions at different times were recorded and analyzed to obtain the ability of heterogeneous inclusions to grow by collision.

[0009] Preferably, the method for preparing the steel containing main inclusions is:

[0010] For materials with Fe as the main matrix, other alloying elements are controlled below 10ppm, and the argon flow rate of high-temperature equipment is reduced to 0-2L·min during the smelting process. -1 , obtaining a steel containing major inclusions with an alloy content between 100-2000ppm.

[0011] Preferably, the preparation method of the secondary inclusions is:

[0012] The secondary inclusions are obtained by preparing pre-melted refined slag using high-temperature equipment, crushing and selecting inclusion particles that meet preset sizes and shapes.

[0013] Preferably, the method for performing high temperature confocal experiment is:

[0014] The high-temperature confocal metallographic furnace is set to a non-vacuum state, steel containing major inclusions and minor inclusions are placed in an alumina crucible, and the alumina crucible is placed horizontally on a platinum-rhodium thermocouple support;

[0015] Adjust the focal length of the high-temperature confocal microscope to make the screen clear, evacuate the gas in the high-temperature confocal metallographic furnace, and repeatedly blow ultrapure argon gas into the furnace three times;

[0016] The melting point of the calcium treated steel is calculated, the temperature is raised at a preset rate based on the melting point, and the collision behavior of heterogeneous inclusions is observed in situ.

[0017] Preferably, heating at a preset rate based on the melting point includes: a first heating, a second heating, and manual temperature adjustment, wherein the first heating is performed at a rate of 200°C·min -1 The heterogeneous inclusions are heated to 1500℃·min -1 The second heating is 10℃·min -1 The temperature was raised to the experimental temperature of 1525°C at a rate of , and then the temperature was manually adjusted until the surface of the molten steel melted.

[0018] Preferably, the argon flow rate is reduced to 2 L min when observing the collision behavior of heterogeneous inclusions in situ. -1 Then turn off the argon flow.

[0019] The present invention also provides a system for studying the collision of heterogeneous inclusions using a high temperature confocal device, which is used to implement the method described, comprising:

[0020] Inclusion preparation module for preparing steel with major inclusions and minor inclusions using high temperature equipment;

[0021] The high temperature confocal experiment module is used to place steel containing major inclusions and minor inclusions in a high temperature confocal metallographic furnace to conduct a high temperature confocal experiment, observe the collision behavior of heterogeneous inclusions in real time, record the positions of inclusions at different times and analyze them to obtain the ability of heterogeneous inclusions to grow by collision.

[0022] Preferably, the high temperature confocal experiment module comprises:

[0023] A sample placing unit, used for making the high temperature confocal metallographic furnace into a non-vacuum state, placing the steel containing the main inclusions and the secondary inclusions in an alumina crucible, and placing the alumina crucible horizontally on a platinum-rhodium thermocouple support;

[0024] The argon purge unit is used to adjust the focal length of the high-temperature confocal microscope to make the screen clear, and to evacuate the gas in the furnace chamber of the high-temperature confocal metallographic furnace, and to purge ultra-pure argon gas into the furnace chamber three times repeatedly;

[0025] The in-situ observation unit is used to calculate the melting point of the calcium-treated steel, increase the temperature at a preset rate based on the melting point, and observe the collision behavior of heterogeneous inclusions in situ.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: the method of the present invention places refined slag on the surface of steel, and then adjusts the temperature to control only the melting of the surface of the molten steel, so as to observe the behavior of the endogenous inclusions on the surface of the steel being adsorbed and collided by the refined slag. Since different refined slags have different adsorption capacities for inclusions in steel, the changes in the collision time and distance of the main inclusions and the secondary inclusions are the focus of the study. The present invention uses new equipment (high temperature confocal microscope) to better control the melting of the molten steel surface, and by simulating the actual slag environment, the adsorption capacity of the refined slag on inclusions is more intuitively analyzed. By studying the adsorption capacity of refined slags of different compositions on inclusions, guidance is provided for actual production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0028] Figure 1 A schematic diagram of a high temperature confocal experiment placement method according to an embodiment of the present invention;

[0029] Figure 2Schematic diagram of the positions of minor inclusions and major inclusions in steel in the experimental method of the embodiment of the present invention;

[0030] Figure 3 This is a diagram showing the position changes of calcium aluminate inclusions (secondary inclusions) and aluminum oxide inclusions (main inclusions) in steel at different times according to an embodiment of the present invention;

[0031] Figure 4 The present invention is a flow chart of a method for studying the collision of heterogeneous inclusions using a high-temperature confocal device. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] Embodiment 1

[0035] like Figure 4 As shown, the method for studying the collision of heterogeneous inclusions using a high temperature confocal device includes the following steps:

[0036] S1: Preparation of steel with major inclusions and minor inclusions using high temperature equipment;

[0037] A further embodiment is that the method for preparing steel containing major inclusions is:

[0038] For materials with Fe as the main matrix, other alloy elements should be controlled below 10ppm to avoid the generation of other types of inclusions during the smelting process, which would affect the observation of the collision behavior of heterogeneous inclusions in the high-temperature confocal experiment. During the smelting process, the argon flow rate of the high-temperature equipment should be reduced to 0-2L·min -1 , obtain steel containing main inclusions with alloy content between 100-2000ppm. The smelting of steel containing a large number of endogenous inclusions requires controlling the generation of a large number of endogenous inclusions in the steel. The alloy content in the steel should be controlled between 100-2000ppm to ensure the generation of a large number of endogenous inclusions in the steel.

[0039] A further embodiment is that the secondary inclusions are prepared by:

[0040] The pre-melted refined slag is prepared by high-temperature equipment. The inclusions separated and extracted from aluminum deoxidized steel by high-temperature melting of a certain proportion of composite oxides or small sample electrolysis experiments need to be controlled at 1.3-1.5 times of its complete melting temperature, and the holding time is controlled at 20-50 minutes to obtain a pre-melted slag with uniform composition. The inclusion particles that meet the preset size and shape are crushed and selected to obtain secondary inclusions. In this embodiment, the size needs to be controlled between 5-500μm.

[0041] S2: The steel containing major inclusions and minor inclusions are placed in a high-temperature confocal metallographic furnace to conduct a high-temperature confocal experiment, observe the collision behavior of heterogeneous inclusions in real time, record the positions of inclusions at different times and analyze the ability of heterogeneous inclusions to grow by collision.

[0042] In this embodiment, a high temperature confocal device model VL2000DX-SVF18SP is used to achieve rapid heating and cooling, with a maximum heating rate of 1000°C min -1 The maximum cooling rate can reach 1500℃·min -1 , which enables in-situ observation of experimental samples at high temperatures.

[0043] A further embodiment is that the method for performing a high temperature confocal experiment is:

[0044] The high-temperature confocal metallographic furnace is set to a non-vacuum state, steel containing major inclusions and minor inclusions are placed in an alumina crucible, and the alumina crucible is placed horizontally on a platinum-rhodium thermocouple support;

[0045] Adjust the focal length of the high-temperature confocal microscope to make the screen clear, evacuate the gas in the high-temperature confocal metallographic furnace, and repeatedly blow ultrapure argon gas into the furnace three times;

[0046] Calculate the melting point of calcium-treated steel, heat it at a preset rate based on the melting point, and observe the collision behavior of heterogeneous inclusions in situ. Specifically, use Factsage thermodynamic software to make a preliminary calculation of the melting point of the experimental steel sample, requiring that when the temperature in the furnace reaches 20K lower than the melting temperature of the molten steel surface, the temperature must be manually adjusted to melt the molten steel surface to avoid heating too quickly, which may cause the loss of minor inclusions on the molten steel surface.

[0047] A further embodiment is that heating according to a preset rate based on the melting point includes: a first heating, a second heating and manual temperature adjustment, wherein the first heating is performed at 200°C·min -1 The heterogeneous inclusions are heated to 1500℃·min -1 The second heating is 10℃·min -1The temperature was raised to the experimental temperature of 1525°C at a rate of , and then the temperature was manually adjusted until the surface of the molten steel melted.

[0048] A further embodiment is to reduce the argon flow rate to 2 L min when observing the collision behavior of heterogeneous inclusions in situ. -1 Then turn off the argon flow to avoid excessive argon flow, which may cause fluctuations in the molten steel and affect the collision behavior of foreign inclusions.

[0049] Embodiment 2

[0050] This example provides a specific inclusion preparation process and a high temperature confocal experiment process:

[0051] S1: Preparation of steel with major inclusions and minor inclusions using high temperature equipment;

[0052] S11: Preparation of steel containing a large amount of alumina inclusions (main inclusions):

[0053] The specific smelting steps of the product containing a large number of main inclusions are as follows: 1) 590g of electrolytic iron is placed in a high-purity Al2O3 crucible with an outer diameter and inner diameter of 60mm and a height of 130mm, and heated to 1873K using a silicon-molybdenum resistance furnace at a heating rate of 50℃·min-1. The Ar flow rate introduced during the entire experiment is 1L·min-1; 2) When the temperature rises to 1873K, it is kept warm for 20min to ensure that the electrolytic iron is completely melted, and then 0.7g of aluminum particles are added from the top of the furnace; 3) After the operation is completed, the crucible sample is water-cooled. The Al-treated steel after water cooling is used as steel containing a large number of aluminum oxide inclusions. Before conducting the high-temperature confocal experiment, the Al-treated steel needs to be processed into a cylinder with a diameter of 5 mm and a height of 3 mm, and polished step by step using sandpaper models 2000#, 500#, and 1200#. After cleaning, the sample is polished using 7μm and 0.5μm polishing liquid, and finally placed in a beaker containing alcohol. The beaker containing the sample is placed in an ultrasonic cleaner for cleaning for 10 minutes.

[0054] S12: Preparation of calcium aluminate inclusions (secondary inclusions):

[0055] The specific preparation steps of calcium aluminate inclusions are as follows: 1) Use an electronic balance to weigh 2g of calcium oxide powder and 2g of aluminum oxide powder, and pour them into a quartz grinding crucible, add alcohol to mix them, and grind them with a grinding rod until the alcohol is completely volatilized, and repeat the operation 3 times. 2) Load the mixed powder into a mold with a diameter of 10mm and press it into shape using a tablet press. 3) Place the pressed powder flakes on an alumina crucible sheet and put it into a muffle furnace. After raising the temperature to 1200℃, keep it warm for 8 hours, and then start cooling at a rate of 100℃·h-1 until it reaches room temperature and then take it out. 4) Crush the powder flakes taken out and take small particles with a diameter of 200μm as secondary inclusions.

[0056] S2: The steel containing major inclusions and minor inclusions are placed in a high-temperature confocal metallographic furnace, and a high-temperature confocal experiment is conducted to observe the collision behavior of heterogeneous inclusions in real time, record the positions of inclusions at different times, and analyze the ability of heterogeneous inclusions to grow by collision.

[0057] Turn on the various devices of the high-temperature confocal microscope. After confirming that the high-temperature heating furnace is in a non-vacuum state, open the furnace cover, place the steel containing the main inclusions and the secondary inclusion particles in an alumina crucible with a diameter of 7.5 mm according to a specific placement method, and place the alumina crucible horizontally on the platinum-rhodium thermocouple holder. The placement method is as follows: Figure 1 As shown. Adjust the focus to make the screen clear, then cover the furnace cover to ensure the sealing of the heating furnace, and then use the vacuum pump to evacuate the gas in the furnace cavity, and then continuously blow ultrapure argon (99.999%) into the furnace cavity, repeating three times to avoid oxidation of the sample surface. During the process of blowing in argon, the valve needs to be adjusted slowly to prevent the sample from being lost due to excessive airflow.

[0058] Before the high temperature confocal experiment, the Phase Diagram module in the FactSage thermodynamics software was selected to calculate the melting point of calcium treated steel to be 1545°C. After the preliminary steps of the experiment were completed, the temperature was set at 200°C min -1 The sample was heated to 1500°C min -1 , then at 10℃·min -1 The temperature will be raised to the experimental temperature of 1525℃ at a rate of , and then it will need to be manually adjusted until the surface of the molten steel melts and insulation observation begins. Figure 2 This is a schematic diagram of the positions of the main and secondary inclusions in the experimental method. It is expected that after the molten steel is melted, the endogenous main inclusions in the steel will approach the secondary inclusions and collide, adsorb and grow. During the experiment, the argon flow needs to be turned off to prevent the argon flow from causing fluctuations on the surface of the molten steel and to avoid the impact of external factors on the collision of inclusions. During the insulation process, high-temperature confocal imaging is used to observe the collision of inclusions on the surface. Figure 3 The following is a graph showing the position changes of calcium aluminate inclusions (secondary inclusions) and alumina inclusions (main inclusions) in steel at different times. By recording the position change of a certain endogenous inclusion, the distance from the main inclusion before the collision and the time required for the collision can be determined to determine the speed at which the alumina inclusion collides with the calcium aluminate inclusion, and then calculate the collision acceleration and adsorption force between the two. Figure 3 Taking the collision between the marked major inclusion and the minor inclusion as an example, the distance between the marked major inclusion in each picture and the final collision position is measured, and recorded as d1, d2, d3, and d4 respectively. In addition, the time of each picture is recorded, and recorded as t1, t2, t3, and t4. Then the average speed of the movement of the major inclusion in the first and second pictures is v1=d1-d2 / t2-t1, and so on. The results are statistically summarized in Table 1.

[0059] Table 1

[0060]

[0061] The adsorption force between the main inclusions and the secondary inclusions at different times is calculated according to the adsorption force formula. The specific formula is shown in 1-1.

[0062]

[0063] Where F is the adsorption force between the major inclusion and the minor inclusion, N; v is the average velocity of the major inclusion movement, m / s; Δt is the interval time between each picture, and its value is approximately 0.5, s; m is the mass of the marked major inclusion, which can be calculated by measuring its radius and density.

[0064] In the past, when using a high-temperature confocal laser scanning microscope to observe the movement of inclusions on the surface of molten steel, it was impossible to determine the composition of the colliding inclusions. At the same time, it was difficult to find the inclusions observed during the experiment to analyze the composition after the experiment. Therefore, the composition of the colliding inclusions could only be roughly determined. However, this method can anchor an inclusion of a certain composition for observation. After the confocal experiment, the composition of other colliding inclusions can also be analyzed by anchoring the inclusion.

[0065] The method of the present invention can be used to study the adsorption capacity of refined slag (secondary inclusions) of different compositions on inclusions (major inclusions) in steel. In the past, the method for studying the ability of refined slag to remove inclusions was based on high-temperature confocal laser scanning microscope equipment to observe the dissolution rate and behavior of inclusions in slag, but this is different from the actual steelmaking environment. This method is to place refined slag (secondary inclusions) on the steel surface, adjust the temperature, and only control the melting of the molten steel surface to observe the behavior of endogenous inclusions (major inclusions) on the steel surface being adsorbed and collided by the refined slag (secondary inclusions). Since different refined slags have different adsorption capacities for inclusions in steel, the changes in the collision time and distance of the main inclusions and secondary inclusions are the focus of the study. The laboratory experiment is used to simulate the adsorption of refined slag on inclusions in the actual production process, and the in-situ observation of the adsorption collision behavior can be realized, which is used to study the adsorption capacity of refined slags of different compositions on inclusions, and has a good guiding significance for actual production.

[0066] Embodiment 3

[0067] The present invention also provides a system for studying the collision of heterogeneous inclusions using a high temperature confocal device, and a method for implementing the system includes:

[0068] Inclusion preparation module for preparing steel with major inclusions and minor inclusions using high temperature equipment;

[0069] The high temperature confocal experiment module is used to place steel containing major inclusions and minor inclusions in a high temperature confocal metallographic furnace to conduct a high temperature confocal experiment, observe the collision behavior of heterogeneous inclusions in real time, record the positions of inclusions at different times and analyze them to obtain the ability of heterogeneous inclusions to grow by collision.

[0070] In a further embodiment, the high temperature confocal experiment module comprises:

[0071] A sample placing unit, used for making the high temperature confocal metallographic furnace into a non-vacuum state, placing the steel containing the main inclusions and the secondary inclusions in an alumina crucible, and placing the alumina crucible horizontally on a platinum-rhodium thermocouple support;

[0072] The argon purge unit is used to adjust the focal length of the high-temperature confocal microscope to make the screen clear, and to evacuate the gas in the furnace chamber of the high-temperature confocal metallographic furnace, and to purge ultra-pure argon gas into the furnace chamber three times repeatedly;

[0073] The in-situ observation unit is used to calculate the melting point of calcium-treated steel, increase the temperature at a preset rate based on the melting point, and observe the collision behavior of heterogeneous inclusions in situ.

[0074] The embodiments described above are only descriptions of the preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for studying the collision of heterogeneous inclusions using a high temperature confocal device, characterized in that: The following steps are involved: Preparation of steel containing major inclusions and minor inclusions using high temperature equipment; The steel containing major inclusions and minor inclusions were placed in a high-temperature confocal metallographic furnace for a high-temperature confocal experiment. The collision behavior of heterogeneous inclusions was observed in real time, and the positions of inclusions at different times were recorded and analyzed to obtain the ability of heterogeneous inclusions to grow by collision.

2. The method for studying the collision of heterogeneous inclusions using a high temperature confocal device according to claim 1, characterized in that: The method for preparing the steel containing main inclusions is: For materials with Fe as the main matrix, other alloying elements are controlled below 10ppm, and the argon flow rate of high-temperature equipment is reduced to 0-2L·min during the smelting process. -1 , obtaining a steel containing major inclusions with an alloy content between 100-2000ppm.

3. The method for studying the collision of heterogeneous inclusions using a high temperature confocal device according to claim 1, characterized in that: The preparation method of the secondary inclusions is: The secondary inclusions are obtained by preparing pre-melted refined slag using high-temperature equipment, crushing and selecting inclusion particles that meet preset sizes and shapes.

4. The method for studying the collision of heterogeneous inclusions using a high temperature confocal device according to claim 1, characterized in that: The method for performing high temperature confocal experiments is: The high-temperature confocal metallographic furnace is set to a non-vacuum state, steel containing major inclusions and minor inclusions are placed in an alumina crucible, and the alumina crucible is placed horizontally on a platinum-rhodium thermocouple support; Adjust the focal length of the high-temperature confocal microscope to make the screen clear, evacuate the gas in the high-temperature confocal metallographic furnace, and repeatedly blow ultrapure argon gas into the furnace three times; The melting point of the calcium treated steel is calculated, the temperature is raised at a preset rate based on the melting point, and the collision behavior of heterogeneous inclusions is observed in situ.

5. The method for studying the collision of heterogeneous inclusions using a high temperature confocal device according to claim 4, wherein heating is performed at a preset rate based on the melting point, comprising: The first heating, the second heating and the manual temperature adjustment, where the first heating is at 200℃·min -1 The heterogeneous inclusions are heated to 1500℃·min -1 The second heating is 10℃·min -1 The temperature was raised to the experimental temperature of 1525°C at a rate of , and then the temperature was manually adjusted until the surface of the molten steel melted.

6. According to the method for studying the collision of heterogeneous inclusions using a high temperature confocal device according to claim 4, when observing the collision behavior of heterogeneous inclusions in situ, the argon gas flow rate is reduced to 2 L·min -1 Then turn off the argon flow.

7. A system for studying the collision of heterogeneous inclusions using a high temperature confocal device, characterized in that: The method for implementing any one of claims 1 to 6 comprises: Inclusion preparation module for preparing steel with major inclusions and minor inclusions using high temperature equipment; The high temperature confocal experiment module is used to place steel containing major inclusions and minor inclusions in a high temperature confocal metallographic furnace to conduct a high temperature confocal experiment, observe the collision behavior of heterogeneous inclusions in real time, record the positions of inclusions at different times and analyze them to obtain the ability of heterogeneous inclusions to grow by collision.

8. The system for studying collision of heterogeneous inclusions using a high temperature confocal device according to claim 7, characterized in that: The high temperature confocal experiment module includes: A sample placing unit, used for making the high temperature confocal metallographic furnace into a non-vacuum state, placing the steel containing the main inclusions and the secondary inclusions in an alumina crucible, and placing the alumina crucible horizontally on a platinum-rhodium thermocouple support; The argon purge unit is used to adjust the focal length of the high-temperature confocal microscope to make the screen clear, and to evacuate the gas in the furnace chamber of the high-temperature confocal metallographic furnace, and to purge ultra-pure argon gas into the furnace chamber three times repeatedly; The in-situ observation unit is used to calculate the melting point of the calcium-treated steel, increase the temperature at a preset rate based on the melting point, and observe the collision behavior of heterogeneous inclusions in situ.