Method for evaluating CVD (Chemical Vapor Deposition) densification effect of carbon-carbon composite material
By selecting perfect circular carbon fibers to measure the pyrolytic carbon thickness of carbon-carbon composite materials, the problem of inaccurate evaluation of the CVD densification effect in the existing technology is solved, semi-quantitative evaluation of the deposition effect is achieved, and the uniformity and performance of the product are improved. Comparability.
Patent Information
- Application Number
- CN202410949636.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-16
AI Technical Summary
It is difficult to effectively evaluate the CVD densification effect of carbon-carbon composite materials with existing technology, resulting in inconsistent deposition effects, reduced air permeability, and impact on product performance. Moreover, traditional measurement methods are not very reliable and cannot be quantitatively compared.
Using a perfect circular carbon fiber as the measurement unit, the thickness of pyrolytic carbon deposited on the surface of the carbon fiber is measured through an optical microscope, and the average pyrolytic carbon thickness ratio between the surface and the middle position is calculated to quantitatively evaluate the CVD densification effect of carbon-carbon composite materials.
It achieves a simple and highly operable semi-quantitative evaluation, improves the accuracy and uniformity of deposition effects, can distinguish different levels of deposition effects, and improves the comparability of product performance.
Smart Images

Figure CN118758934A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material preparation effect detection, and in particular relates to a method for evaluating the CVD densification effect of a carbon-carbon composite material. Background Art
[0002] Carbon-carbon composite materials not only have excellent structural material properties such as high specific strength and high specific modulus, but also have excellent thermophysical properties. They can well meet the comprehensive performance requirements of the aerospace industry for materials under high temperature and high speed conditions, and have been applied to the new generation of aerospace material brake discs. Among them, carbon-carbon composite materials are a composite material with carbon fiber as the skeleton and matrix carbon densified on the carbon fiber. The entire system is composed of carbon elements and is a multiphase inhomogeneous mixture in terms of fiber structure. The mechanical properties, thermophysical properties and friction and wear properties of this material are closely related to the composition of the material.
[0003] The matrix carbon of carbon-carbon composite materials is mainly formed in the CVD process, among which the isothermal CVD technology (ICVI) can be simple in ICVI process, not limited by the geometric size of the product, with good process repeatability, and can achieve mass production. In addition, the prepared deposited carbon can obtain a uniform rough layer of pyrolytic carbon, the product quality and performance are good, and the friction coefficient of the product is less attenuated under high energy load conditions. It is an ideal means of matrix carbon deposition. However, since the deposition process is greatly affected by the gas diffusion efficiency, the permeability of the material gradually decreases with the deposition of ICVI matrix carbon, which greatly affects the deposition rate of ICVI. This leads to inconsistent deposition effects.
[0004] Although ICVI technology is relatively mature at home and abroad, there are still differences in the details of ICVI key technologies of different manufacturers at home and abroad (raw materials, gas flow, deposition time, deposition temperature, etc.). Different process routes lead to certain differences in the deposition effect of the matrix carbon. Due to the different thicknesses of different products, the deposition effect also varies greatly. Some carbon-carbon composite materials have more carbon deposited on the surface, resulting in a higher density of the surface product, while the deposited carbon content in the middle is lower, resulting in a lower density in the middle; some carbon-carbon composite materials have large sizes, and there are also large differences in the deposition effect and deposition density inside, in the middle, and outside. Therefore, evaluating the overall deposition effect of the matrix carbon of a carbon-carbon composite material has become an important method for evaluating ICVI production effects and even product performance.
[0005] Currently, the evaluation of the deposition effect of matrix carbon is mainly based on observing the cross-section metallographic diagram, and measuring the degree of anisotropy by measuring the reflection of polarized light by pyrolytic carbon and the size of the extinction angle. However, due to the large recognition error in measuring the extinction angle, the credibility of this evaluation method is not high. It can only qualitatively evaluate whether the product is a rough layer, a smooth layer, etc., and cannot quantitatively or semi-quantitatively compare between products. Summary of the invention
[0006] In view of the shortcomings of the prior art, the object of the present invention is to provide a method that is simple, highly operable and can semi-quantitatively evaluate the CVD densification effect of carbon-carbon composite materials.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The present invention discloses a method for evaluating the CVD densification effect of a carbon-carbon composite material. The method comprises the following steps: firstly cutting a long block having a height equal to the thickness of the carbon-carbon composite material along the span of the carbon-carbon composite material, and then segmenting the long block along the original span direction and the thickness direction to obtain a plurality of block samples. The block samples are all prepared according to the test requirements of an optical microscope to obtain a test sample. The test sample is placed on an optical microscope, and the cut surface of the original carbon-carbon composite material is used as the observation surface. The surface and the middle of the test sample are selected for measurement at observation points. Among the observation points, a circular carbon fiber is selected as a measurement unit to measure the thickness of pyrolytic carbon deposited on the surface of the carbon fiber. Finally, based on the measurement results, the CVD densification effect of the carbon-carbon composite material is evaluated. When the surface average pyrolytic carbon thickness is ≥18 μm and the middle average pyrolytic carbon thickness is: the surface average pyrolytic carbon thickness is >0.8, the test sample is classified as Grade I. When the surface average pyrolytic carbon thickness is ≥18 μm and the middle average pyrolytic carbon thickness is: the surface average pyrolytic carbon thickness is 0.6-0.8, the test sample is classified as Grade II. , when the average pyrolytic carbon thickness on the surface is ≥18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is <0.6, it is Class III; when the average pyrolytic carbon thickness on the surface is 16-18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is >0.8, it is Class II; when the average pyrolytic carbon thickness on the surface is 16-18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is 0.6-0.8, it is Class III; when the average pyrolytic carbon thickness on the surface is 16-18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is 0.6-0.8, it is Class III; When the thickness is 16-18μm and the average middle pyrolytic carbon thickness: the average surface pyrolytic carbon thickness is <0.6, it is Grade IV; when the average surface pyrolytic carbon thickness is 12-16μm and the average middle pyrolytic carbon thickness: the average surface pyrolytic carbon thickness is >0.8, it is Grade III; when the average surface pyrolytic carbon thickness is 12-16μm and the average middle pyrolytic carbon thickness: the average surface pyrolytic carbon thickness is ≤0.8, it is Grade IV; when the average surface pyrolytic carbon thickness is ≤12, it is Grade IV.
[0009] The present invention provides a method for evaluating the CVD densification effect of a carbon-carbon composite material. By selecting a perfectly circular carbon fiber as an observation unit and measuring the thickness of the deposited carbon deposited on the pyrolytic carbon, the CVD densification effect of the carbon-carbon composite material can be semi-quantitatively evaluated. The inventors have found that only by selecting a perfectly circular carbon fiber as the measurement unit at the observation point can the result be accurately evaluated. If the carbon fiber is not a perfectly circular carbon fiber, the test result will be affected because the cross-section is not a vertical plane.
[0010] The method for evaluating the CVD densification effect of the carbon-carbon composite material of the present invention is to quantitatively obtain the deposited carbon thickness of a single carbon fiber deposited in the carbon-carbon composite material, and calculate the average pyrolytic carbon thickness ratio of the middle position of the cut surface of the carbon-carbon composite material and the surface average pyrolytic carbon to quantitatively evaluate the CVD densification effect. In the present invention, grade I is better than grade II, grade III is better than grade IV, that is, the thicker the surface average pyrolytic carbon thickness, the greater the ratio of the middle average pyrolytic carbon thickness to the surface average pyrolytic carbon thickness, the better. The greater the ratio of the middle average pyrolytic carbon thickness to the surface average pyrolytic carbon thickness, the smaller the gap between the middle and the surface, and the better the uniformity.
[0011] In a preferred solution, a long block having a width of 18-22 mm and a height equal to the thickness of the carbon-carbon composite material is cut along the span of the carbon-carbon composite material.
[0012] After the block is made into a test sample, the cut cross section is the surface to be observed, and it is necessary to control the surface to be observed to be smooth and flat.
[0013] In a preferred embodiment, the length of the block sample is 20-30 mm and the height is 5-10 mm. In the present invention, the length direction of the block sample is the distance measured in the span direction of the original carbon-carbon composite material, and the height is the distance measured along the thickness direction of the carbon-carbon composite material. When cutting, the edges are neat and the surface is flat. After the sample is segmented, it is marked from inside to outside and from left to right.
[0014] According to a preferred embodiment, the sample preparation process is as follows: a block sample is placed in a mold, and then liquid epoxy resin is injected. After curing, the sample is polished to obtain the sample. The liquid epoxy resin is composed of epoxy resin, butylene phthalate, and ethylenediamine.
[0015] In the present invention, the optical microscope test requires the following sample preparation process: a block sample is placed in a cylindrical plastic mold coated with a release agent (vaseline), and then the mold is placed in a vacuum device to evacuate the vacuum to a degree of 9.1 to 9.5 × 10 4Pa, turn off the vacuum pump and the air inlet valve, and inject liquid epoxy resin from the top of the device to cover the sample by about 3mm. Take out the sample and solidify it in the air after about 1 hour. Before injecting the resin, 1 / 4 of the weight of the resin should be added to the resin as a solvent to dissolve the resin into a liquid state; then add 1 / 12 of the weight of the resin as a curing agent to harden the resin. After polishing the sample, fine-polish the sample with 2.5μm and 1μm alumina suspension. After fine polishing, the sample should be smooth and traceless. No fine scratches should be observed under a 100× microscope, and there should be no tailing phenomenon. The pores are fully displayed and reflect the true appearance.
[0016] Preferably, the optical microscope is equipped with a polarizer and a rotatable analyzer.
[0017] In a preferred solution, the carbon fibers are independent carbon fibers. The inventors have found that the carbon fibers should be relatively independent and clustered carbon fibers should not be selected, otherwise the results will be affected.
[0018] The preferred solution is that the selection of the observation points is still based on the positioning of the long block, the distance between adjacent observation points on the control surface is between 20 and 30 mm, the observation points in the middle area should be between 10 mm above and below the thickness center line, preferably between 5 mm, and the distance between adjacent observation points in the middle area is between 20 and 30 mm.
[0019] In a preferred embodiment, at any observation point, at least three perfectly circular carbon fibers are selected as measurement units.
[0020] Beneficial Effects
[0021] The method for evaluating the CVD densification effect of carbon-carbon composite materials of the present invention selects perfectly circular carbon fibers as observation units and measures the thickness of deposited carbon deposited on pyrolytic carbon, thereby semi-quantitatively evaluating the CVD densification effect of carbon-carbon composite materials. The test method is relatively simple and has strong operability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Example 1 Sampling schematic diagram;
[0023] Figure 2 Schematic diagram of the positional relationship of segmenting a long block in Example 1;
[0024] Figure 3 Schematic diagram of observation point locations based on the long block in Example 1;
[0025] Figure 4 Schematic diagram of observation point locations based on the long block in Example 1;
[0026] Figure 5Metallographic structure diagram of the surface and middle observation points in Example 1.
[0027] Figure 6 Metallographic structure diagram of the surface and middle observation points in Example 2.
[0028] Figure 7 Metallographic structure diagram of the surface and middle observation points in Example 3.
[0029] Figure 8 Metallographic structure diagram of the measurement points of carbon fibers with different morphologies in Comparative Example 1, where Figure 8 A is the metallographic structure of a circular carbon fiber measurement point. Figure 8 B is the metallographic structure diagram of the non-circular carbon fiber measurement point. DETAILED DESCRIPTION
[0030] Example 1
[0031] 1. Sampling
[0032] Use a cutting machine to take a rectangular spline with a span length of 75mm, a width of 20mm, and a height of 24mm along the radial span of the carbon disk. The sampling diagram is shown in the figure. Figure 1 As shown, the cross section of the spline sample along the radial direction is the observation surface, and the observation surface should be smooth and flat; the number of spline segments is determined according to the span size of the carbon disk, and the segmentation diagram is shown in Figure 2 As shown, each sample is 25 mm long and 8 mm high, with neat edges and a flat surface. A total of 6 surface and middle block samples were obtained. After the samples were segmented, they were marked from the inner diameter to the outer diameter.
[0033] The sample was placed in a cylindrical plastic mold coated with a release agent (vaseline), and the mold was placed in a vacuum device to evacuate the sample to a vacuum degree of 9.1 to 9.5 × 10 4 Pa, turn off the vacuum pump and the air inlet valve, and inject liquid epoxy resin from the top of the device to cover the sample by about 3mm. Take out the sample and solidify it in the air after about 1 hour. Before injecting the resin, 1 / 4 of the weight of the resin should be added to the resin as a solvent to dissolve the resin into a liquid state; then add 1 / 12 of the weight of the resin as a curing agent to harden the resin. After polishing the sample, fine-polish the sample with 2.5μm and 1μm alumina suspension. After fine polishing, the sample should be smooth and traceless. No fine scratches should be observed under a 100× microscope, and there should be no tailing phenomenon. The pores are fully displayed and reflect the true appearance.
[0034] 2. Measurement
[0035] All measurements were performed on an optical microscope equipped with a polarizer and a rotatable analyzer. Figure 3 , Figure 4 The measurement position should be evaluated on the surface and the middle of the carbon disc, the surface observation point should be between 20 and 30 mm, the middle area observation point should be in the middle of the sample, and the adjacent observation points should be between 20 and 30 mm.
[0036] Among the observation points, a circular carbon fiber (the cross section of a non-circular carbon fiber is not a vertical plane) is selected as the measurement unit, and the thickness of the deposited carbon deposited on the pyrolytic carbon is measured; the selected carbon fiber should be relatively independent, and clustered carbon fibers should not be selected, otherwise the results will be affected; the observation point range should cover representative parts from the inner diameter to the outer diameter, and from the surface to the center, as shown in Table 2.
[0037] 3. Collect and analyze statistical data;
[0038] Then, according to the test results, the product matrix carbon deposition quality - the thickness of the deposited carbon is evaluated. The metallographic diagram and results of the carbon disc pyrolysis carbon in Example 1 Figure 5 As shown in Table 2. The average thickness of the surface pyrolytic carbon is 18.53 μm, the thickness of the middle pyrolytic carbon: the thickness of the surface pyrolytic carbon = 0.81, according to the evaluation results in Table 1, the product grade is Grade I.
[0039] Table 1 Product pyrolysis carbon deposition carbon deposition effect judgment standard
[0040]
[0041]
[0042] Table 2 Carbon deposition thickness at each location in Example 1
[0043]
[0044] Example 2
[0045] Due to production problems, a company produced a batch of faulty products B. The sampling method was the same as in Example 1. The random sampling of the surface and the middle section was obtained by this technology. The statistical data was collected and analyzed to evaluate the carbon deposition quality of the product matrix - the thickness of the deposited carbon. The metallographic diagram and results of the carbon disc pyrolysis carbon in Example 1 Figure 6 As shown in Table 3. The average thickness of pyrolytic carbon on the surface of product B is less than 12 μm. According to the evaluation criteria, the product grade is IV.
[0046] Table 3 Carbon deposition thickness at each part of product B
[0047]
[0048] Example 3
[0049] The CVD densification effect of product C carbon disk produced by a company is evaluated. The sampling method is the same as in Example 1. The statistical data is collected and analyzed to evaluate the carbon deposition quality of the product matrix - the thickness of the deposited carbon. The metallographic phase diagram and results of product C pyrolytic carbon in Example 3 Figure 7 As shown in Table 4. The average thickness of the surface pyrolytic carbon is 18.52 μm, and the surface pyrolytic carbon thickness / intermediate pyrolytic carbon thickness = 0.78. According to the evaluation results in Table 1, the product grade is II.
[0050] Table 4 Carbon deposition thickness at each part of a sample
[0051]
[0052] Comparative Example 1:
[0053] In the observation unit, the circular carbon fiber is selected as the measurement unit to accurately evaluate the results. If the carbon fiber is not circular, the test results will be affected because the cross section is not a vertical plane. Figure 8 As shown, A is a perfect circular carbon fiber, and the metallographic thickness of the product is relatively uniform (such as Figure 8 A), the metallographic thickness is about 13.83μm. If the non-circular B is selected as the measurement unit, the measurement results will be quite different (such as Figure 8 B), the actual measurement result range is 12.88μm~16.09μm, which leads to inaccurate product performance.
[0054] In addition, during the actual exploration process, the inventors found that the carbon fibers should be selected relatively independently, and clustered carbon fibers should not be selected, otherwise it will also affect the results.
Claims
1. A method for evaluating the CVD densification effect of carbon-carbon composite materials, Features: First, a long block with a height equal to the thickness of the carbon-carbon composite material is cut along the span of the carbon-carbon composite material, and then the long block is segmented along the original span direction and the thickness direction to obtain a number of block samples. The block samples are all prepared according to the test requirements of the optical microscope to obtain test samples, and the test samples are placed on the optical microscope. The cut surface of the original carbon-carbon composite material is used as the observation surface, and the surface and middle observation points of the test sample are selected for measurement. Among the observation points, a perfect circular carbon fiber is selected as the measurement unit to measure the thickness of the pyrolytic carbon deposited on the surface of the carbon fiber. Finally, according to the measurement results, the CVD densification effect of the carbon-carbon composite material is evaluated. When the surface average pyrolytic carbon thickness is ≥18μm and the middle average pyrolytic carbon thickness: the surface average pyrolytic carbon thickness is>0.8, it is level I, when the surface average pyrolytic carbon thickness is ≥18μm and the middle average pyrolytic carbon thickness: the surface average pyrolytic carbon thickness is 0.6-0.8, it is level II, and when the surface average pyrolytic carbon thickness is ≥18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is <0.6, it is Class III; when the average pyrolytic carbon thickness on the surface is 16-18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is >0.8, it is Class II; when the average pyrolytic carbon thickness on the surface is 16-18μm, and the average pyrolytic carbon thickness in the middle: the average pyrolytic carbon thickness on the surface is 0.6-0.8, it is Class III; when the average pyrolytic carbon thickness on the surface is 16-1 8μm, and the middle average pyrolytic carbon thickness: the surface average pyrolytic carbon thickness is <0.6, it is Level IV; when the surface average pyrolytic carbon thickness is 12-16μm, and the middle average pyrolytic carbon thickness: the surface average pyrolytic carbon thickness is >0.8, it is Level III; when the surface average pyrolytic carbon thickness is 12-16μm, and the middle average pyrolytic carbon thickness: the surface average pyrolytic carbon thickness is ≤0.8, it is Level IV; when the surface average pyrolytic carbon thickness is ≤12, it is Level IV.
2. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Features: A long block with a width of 18-22 mm and a height equal to the thickness of the carbon-carbon composite material is cut along the span of the carbon-carbon composite material.
3. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Features: The block sample has a length of 20-30 mm and a height of 5-10 mm.
4. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Features: The sample preparation process is as follows: a block sample is placed in a mold, and then liquid epoxy resin is injected, and after solidification, the sample is polished to obtain the sample. The liquid epoxy resin is composed of epoxy resin, butylene phthalate, and ethylenediamine.
5. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Claims Features: The optical microscope is equipped with a polarizer and a rotatable analyzer.
6. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Features: The carbon fibers are independent carbon fibers.
7. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1, Features: The selection of the observation points is still based on the positioning of the long block. The distance between adjacent observation points on the control surface is between 20 and 30 mm. The observation points in the middle area should be between 10 mm above and below the thickness center line, and the distance between adjacent observation points in the middle area is between 20 and 30 mm.
8. A method for evaluating the CVD densification effect of carbon-carbon composite materials according to claim 1 or 7, Features: At any observation point, select at least 3 perfectly circular carbon fibers as measurement units.
Citation Information
Patent Citations
Carbon-ceramic material as well as preparation method and application thereof
CN112266258A
Method for testing high-temperature mechanical properties of carbon fibers
CN112858034A
Method for rapidly preparing carbon / carbon composite material brake disc
CN115819101A
Preparation method of carbon / carbon-silicon carbide composite material
CN116332663A
Method for measuring interlayer density of carbon fiber-containing preform material
CN116380712A