Method for preparing ferric oxide-based supercapacitor negative electrode material through thermal shock
Modification of iron oxide-based supercapacitor negative electrode materials by thermal shock method solves the problems of insufficient conductivity and cycle stability, achieves higher electrochemical performance and stability, and is suitable for negative electrode materials of supercapacitors.
Patent Information
- Application Number
- CN202411000425.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
AI Technical Summary
Iron oxide (Fe2O3), as the negative electrode material of supercapacitors, has poor electrical conductivity and poor cycle stability, resulting in poor electrochemical performance.
The thermal shock method is used to treat iron oxide-based materials to improve electrical conductivity and electrochemical performance by changing their microstructure, refining grains, and increasing grain boundaries and defect levels. Specific steps include uniformly stirring the iron salt and solvent to form a precursor solution, immersing the substrate and then performing direct current non-equilibrium thermal shock treatment in a vacuum environment, and adjusting the temperature and time to form a mesoporous structure.
The electrochemical performance of the iron oxide-based supercapacitor negative electrode material is improved, the voltage window is expanded, and ion transport is accelerated. The material has high stability, simple synthesis equipment, and easy operation, making it suitable for use as a self-supporting electrode.
Smart Images

Figure CN118762940A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of supercapacitors, and in particular relates to a method for preparing an iron oxide-based supercapacitor negative electrode material through thermal shock. Background Art
[0002] Iron oxide (Fe2O3) is abundant on Earth, inexpensive, and has a stable and wide operating window at negative potentials. The theoretical specific capacitance of iron oxide (Fe2O3) is higher than that of traditional carbon-based negative electrode materials, making it suitable as a high-performance negative electrode material for supercapacitors. However, Fe2O3 itself has poor conductivity and poor cycle stability, and has the disadvantage of poor electrochemical performance.
[0003] Based on this, a method for preparing iron oxide-based supercapacitor negative electrode materials by thermal shock is needed, which can change the microstructure of Fe2O3 by thermal shock, refine the grains, increase the grain boundaries, increase the degree of defects, expand the ion channels, accelerate ion transmission, improve conductivity, and thus improve its electrochemical performance. Summary of the invention
[0004] In order to solve the problem of poor electrical conductivity of iron oxide materials, the present invention provides a method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock.
[0005] The present invention relates to a method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock, comprising the following steps:
[0006] Step 1: adding iron salt to the solvent and stirring evenly to obtain a precursor solution;
[0007] Step 2, immersing the substrate in the precursor solution, taking out the substrate and drying it to obtain an immersed substrate;
[0008] Step 3: In a vacuum environment, the substrate impregnated in step 2 is subjected to thermal shock treatment by a non-equilibrium thermal shock method using direct current, and after cooling, a thermally-shock-modified supercapacitor negative electrode material is obtained.
[0009] Furthermore, in step 1, the iron salt is one of chloride, nitrate or sulfate, and the solvent is anhydrous ethanol.
[0010] Furthermore, in step 1, the concentration of the iron salt in the precursor solution is 0.5 mol / L to 1.5 mol / L.
[0011] Furthermore, in step 2, the substrate is carbon cloth.
[0012] Furthermore, in step 2, the substrate is immersed in the precursor solution for 0.5 h to 5 h.
[0013] Furthermore, in step 2, the substrate is taken out and then dried in an air atmosphere for 1 to 2 hours.
[0014] Furthermore, in step three, the adjustment range of the direct current is: voltage is 5V to 50V, and current is 5A to 50A.
[0015] Furthermore, in step three, the time for thermal shock treatment of the substrate after immersion in step two is 0.1s to 5s.
[0016] Furthermore, in step three, the temperature threshold of the thermal shock treatment is 800°C to 1200°C.
[0017] Furthermore, in step three, the heating rate of the thermal shock is 1000°C / s to 2000°C / s, and the cooling rate is 1000°C / s to 2000°C / s.
[0018] Beneficial Effects
[0019] The present invention proposes a method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock. The Fe2O3 material prepared by the method has a mesoporous structure in the crystal, increases the interplanar spacing, makes the material produce a wider voltage window, increases the oxygen vacancy content, thereby accelerating ion transport and improving electrochemical performance. At the same time, the material synthesis equipment is simple, easy to operate, and does not rely on component regulation. The electrode material prepared by the present invention has a self-supporting substrate and can be used as an electrode without additional coating. The material has high stability and broad prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a test curve chart of the constant current charge and discharge test (GCD) of the iron oxide-based supercapacitor negative electrode material based on thermal shock modification prepared in Examples 1 to 5 of the present invention.
[0021] Figure 2 The test curve diagram is a cyclic voltammetry (CV) test of the iron oxide-based supercapacitor negative electrode material based on thermal shock modification prepared in Examples 1 to 5 of the present invention. DETAILED DESCRIPTION
[0022] The following combination Figures 1 to 2 This embodiment will be described in detail.
[0023] The present invention relates to a method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock, comprising the following steps:
[0024] Step 1: Add iron salt to the solvent and stir evenly to obtain a precursor solution.
[0025] The iron salt is one of chloride, nitrate or sulfate, the solvent is anhydrous ethanol, and the concentration of the iron salt in the precursor solution is 0.5 mol / L to 1.5 mol / L.
[0026] Step 2: immerse the substrate in the precursor solution, take out the substrate and dry it to obtain an immersed substrate.
[0027] The substrate is carbon cloth, and the substrate is immersed in the precursor solution for 0.5 hours to 5 hours. After the substrate is taken out, it is dried in an air atmosphere, and the drying time is 1 hour to 2 hours.
[0028] Step 3: In a vacuum environment, the substrate impregnated in step 2 is subjected to thermal shock treatment by a non-equilibrium thermal shock method using direct current, and after cooling, a thermally-shock-modified supercapacitor negative electrode material is obtained.
[0029] Direct current refers to direct current with a voltage of 5V to 50V and a current of 5A to 50A.
[0030] The time for thermal shock treatment of the substrate after impregnation in step 2 is 0.1s to 5s, the temperature threshold of thermal shock treatment is 800℃ to 1200℃, the heating rate of thermal shock is 1000℃ / s to 2000℃ / s, and the cooling rate is 1000℃ / s to 2000℃ / s.
[0031] Embodiment 1
[0032] Step 1: Prepare a precursor solution with FeCl3 as solute and anhydrous ethanol as solvent at a concentration of 1 mol / L.
[0033] Step 2: At room temperature, a 1 cm × 3 cm carbon cloth is used as a substrate and immersed in the precursor solution for 0.5 h. After being taken out, it is dried in an air atmosphere for 1 h to obtain an immersed substrate;
[0034] Step 3: In a vacuum environment, a voltage of 20V and a current of 5A, the temperature threshold is set to 800°C, and the impregnated substrate is subjected to a non-equilibrium thermal shock method for 2s using direct current. After cooling, a thermally-shocked supercapacitor negative electrode material, namely, Fe2O3-based oxide, is obtained. The heating rate of the thermal shock is about 1000°C / s, and the cooling rate is about 1000°C / s.
[0035] Embodiment 2
[0036] The difference between this embodiment and the first embodiment is that the temperature threshold in step 3 is 900° C. The rest is the same as the first embodiment.
[0037] Embodiment 3
[0038] The difference between this embodiment and the first embodiment is that the temperature threshold in step 3 is 1000° C. The rest is the same as the first embodiment.
[0039] Embodiment 4
[0040] The difference between this embodiment and the first embodiment is that the temperature threshold in step 3 is 1100° C. The rest is the same as the first embodiment.
[0041] Embodiment 5
[0042] The difference between this embodiment and the first embodiment is that the temperature threshold in step 3 is 1200° C. The rest is the same as the first embodiment.
[0043] Embodiment 6
[0044] The difference between this embodiment and the second embodiment is that the heat shock treatment time in step 3 is 1 second. The rest is the same as the second embodiment.
[0045] Embodiment 7
[0046] The difference between this embodiment and the second embodiment is that the heat shock treatment time in step 3 is 5 seconds. The rest is the same as the second embodiment.
[0047] Compared with the first embodiment, the second to fifth embodiments adjust the degree of lattice strain by changing the temperature threshold of thermal shock.
[0048] Compared with the first embodiment, the sixth and seventh embodiments adjust the lattice strain degree by changing the power-on time.
[0049] Figure 1 The test curve diagram of the constant current charge and discharge test (GCD) of the iron oxide-based supercapacitor negative electrode material based on thermal shock modification prepared in Examples 1 to 5 of the present invention shows good symmetry, indicating that the coulomb efficiency is relatively high during the charge and discharge process.
[0050] Figure 2 The test curve of the cyclic voltammetry (CV) test of the iron oxide-based supercapacitor negative electrode material based on thermal shock modification prepared in Examples 1 to 5 of the present invention. According to the data of the curve, it can be calculated that the mass specific capacitance of Fe2O3-1000℃ is 26F·g -1 .
[0051] The above contents of the present invention are only preferred embodiments of the present invention and are not intended to limit the implementation scheme of the present invention. A person skilled in the art can easily make corresponding changes or modifications based on the main concept and spirit of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope required by the claims.
Claims
1. A method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock, It is characterized in that The steps include: Step 1: adding iron salt to the solvent and stirring evenly to obtain a precursor solution; Step 2, immersing the substrate in the precursor solution, taking out the substrate and drying it to obtain an immersed substrate; Step 3: In a vacuum environment, the substrate impregnated in step 2 is subjected to thermal shock treatment by a non-equilibrium thermal shock method using direct current, and after cooling, a thermally-shock-modified supercapacitor negative electrode material is obtained.
2. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step 1, the iron salt is one of chloride, nitrate or sulfate, and the solvent is anhydrous ethanol.
3. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step 1, the concentration of the iron salt in the precursor solution is 0.5 mol / L to 1.5 mol / L.
4. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step 2, the substrate is carbon cloth.
5. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step 2, the substrate is immersed in the precursor solution for 0.5 h to 5 h.
6. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step 2, the substrate is taken out and then dried in an air atmosphere for 1 to 2 hours.
7. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step three, the adjustment range of the direct current is: voltage is 5V to 50V, and current is 5A to 50A.
8. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step three, the substrate impregnated in step two is subjected to thermal shock treatment for a period of 0.1s to 5s.
9. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step three, the temperature threshold of the thermal shock treatment is 800°C to 1200°C.
10. The method for preparing an iron oxide-based supercapacitor negative electrode material by thermal shock according to claim 1, It is characterized in that In step three, the heating rate of the thermal shock is 1000°C / s to 2000°C / s, and the cooling rate is 1000°C / s to 2000°C / s.
Citation Information
Cited By
Method for constructing heterostructure based on thermotropic electron transfer
CN119392301A