Increased density powder mixtures for additive manufacturing
By mixing particle fractions A, B, and C with different median particle sizes in additive manufacturing to form a high-density powder mixture, the problem of density reduction and mechanical property damage caused by the small particle size distribution of powders in additive manufacturing is solved, and a more efficient solution is achieved. High productivity and lower defect count.
Patent Information
- Application Number
- CN202380024022.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-29
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-11
AI Technical Summary
In the additive manufacturing process, the small particle size distribution of conventional powders leads to reduced layer thickness after consolidation, gas trapping leading to reduced density and damage to mechanical properties, and it is difficult to achieve density optimization in conventional AM processing machines with existing methods.
By mixing three particle fractions A, B and C with different median particle sizes, it is ensured that the median particle sizes of the particle fractions are related to each other, resulting in a high-density powder mixture that provides better processing characteristics and productivity.
A compromise between high density and processability found in conventional additive manufacturing is achieved, reducing the number of defects, increasing productivity, and reducing surface roughness.
Smart Images

Figure CN118765221A_ABST
Abstract
Description
[0001] The invention relates to a powder mixture for additive manufacturing, comprising three particle fractions A, B and C with different median particle sizes, wherein the median particle sizes are related to each other by 0.2-0.5 / 1 / 1.2-2. The invention further relates to a method for preparing a corresponding powder mixture, a method and a device for preparing a three-dimensional object from such a powder mixture, and a correspondingly prepared three-dimensional object, as well as the use of the powder mixture for reducing the number of defects in an additive manufacturing process. Prior art
[0002] Direct Metal Laser Sintering (DMLS) is a laser-based rapid prototyping and tooling method by which net-shape parts are manufactured in a single process. Complex parts can be produced directly from 3D-CAD models by solidifying metal powder layers layer by layer in sections corresponding to the cross-section of the three-dimensional part in the corresponding layer. This method is described in detail, for example, in Juha Kotila et al., Steel-based Metal Powder Blend for Direct Metal Laser Sintering Process, Advances in Powder Metallurgy & Particular Materials, 1999, Vol. 2, Part 5, pp. 87-93; and T. et al., New Innovations in Direct Metal Laser Sintering Process—A Step Forward in Rapid Prototyping and Manufacturing, Laser Materials Processing, Vol. 87, 1999, pp. 68-76.
[0003] For example, EP 1 762 122 A1 discloses a method for producing three-dimensional objects by selective laser sintering or selective laser melting and an apparatus for carrying out this method.
[0004] During processing by layer-by-layer solidification, a layer of powder material is spread out on a support or a previous layer already produced in the process, after which, in a second step, parts of the layer intended to produce the object later are consolidated. For technical reasons, the corresponding powders are often prepared as powders with a relatively small particle size distribution, which ensures the desired processing characteristics of the spread powder layer. In these powders, due to the particle form, the density of the material is significantly lower than the density of the material after consolidation. Therefore, consolidation often leads to a reduction in the thickness of the layer after consolidation.
[0005] In a powder layer, the volume not occupied by particles is often filled with a gas, such as ambient air or, if processed under an inert gas, under a corresponding gas. After melting, this gas is usually vented to the atmosphere, but in some cases can become trapped in the layer in the form of bubbles and defects, which reduce the density of the object produced therefrom and can impair its desired mechanical properties. Therefore, there is a need for a method of processing powders by additive manufacturing that minimizes and reduces the number of defects caused by gases trapped in the object during its production. In addition, the gas causes a loss of energy during melting, since some of the heat is absorbed by the gas, which leads to a loss of productivity.
[0006] In addition, defects may also occur due to uneven melting resulting from irradiation in the consolidation step. Here, the problem is that although the material is evenly dispersed from a macroscopic point of view, the amount of material can vary significantly at the microscopic level. For example, when the thickness of the other layers applied stacked on each other is 60 μm, the 60 μm as a whole can be occupied by two particles with a thickness of 30 μm or one particle with a thickness of 35 μm, with the remaining space filled with gas. In the case of significantly different energy / solid volume ratios after irradiation (with the same power), and correspondingly, the part with less material can be heated to a higher temperature than the part with more material. This in turn leads to differences in cooling and solidification behavior, which can lead to different final properties on the μm scale.
[0007] Although these problems are often addressed by adjusting the processing conditions, there is currently no way to completely avoid them.
[0008] An obvious way to circumvent the problems indicated above is to increase the density of the powder, as this will reduce the amount of gas in each layer before consolidation and increase the uniformity of the amount of material on the μm scale.
[0009] One method capable of increasing the packing density of powders for additive manufacturing and other processes is described in WO 2015 / 073081. According to this document, the size and ratio of two or more main powders with different average particle sizes are calculated to achieve optimal utilization of the space. In an example, WO 2015 / 073081 describes, for example, a granular powder with a residual gas filling volume of only about 18%, which is obtained by mixing two Ti6-4 highly spherical granular powders with effective median particle sizes of about 25 μm and 1 μm in a ratio of 71 / 29. However, in this case, WO 2015 / 073081 reports that the particles tend to phase separate and that the final density is highly dependent on the processing conditions.
[0010] In additive manufacturing, the particles to be processed are often applied from containers or storage systems, where adjusting the conditions to achieve an optimal density is difficult to achieve. In addition, because the powder must be applied as a layer, the particle mixture must also have suitable properties in terms of flowability and achievable uniformity of the layer produced from the powder.
[0011] Therefore, there is a need for an optimized powder that has increased density relative to conventional powders but can actually be used in conventional additive manufacturing (AM) processing machines.
[0012] The present application addresses these needs. Summary of the invention
[0013] In the present research, it has been unexpectedly found that a powder of increased density (relative to conventional powders used for example for laser sintering) can be obtained by mixing three initial powders each having a different median particle size and wherein the particle sizes differ from each other by a limited amount. Although the mixture is not optimized for maximum density, the powder provides better processing characteristics than density-optimized powders and can therefore replace conventional powders in additive manufacturing processes without complex modifications to the equipment. Nevertheless, the increased density allows the use of higher energy inputs during melting, which provides an increase in productivity.
[0014] Thus, in a first aspect, the present invention relates to a powder mixture for use in an additive manufacturing process, wherein the powder mixture comprises a particle fraction A having a median particle size α, a particle fraction B having a median particle size β less than the median particle size α, and a particle fraction C having a median particle size γ greater than the average particle size α, wherein the median particle sizes of the particle fractions B, A and C are related to each other in the range of 0.2-0.5 / 1 / 1.2-2. Preferably, the median particle sizes of the particle fractions B, A and C are related to each other in the range of 0.2-0.5 / 1 / 1.3-2, more preferably 0.25-0.4 / 1 / 1.5-1.8, even more preferably 0.3-0.4 / 1 / 1.5-1.8, and even more preferably the median particle sizes are related to each other in the range of about 1 / 3 / 1 / 5 / 3.
[0015] The “median particle size” of the corresponding particle fraction is the D50 particle size determined by laser diffraction according to ISO 13320:2020, where half of the particles (according to their volume) are smaller than D50 and half are larger than D50.
[0016] The median particle size of the corresponding fractions A, B and C can be determined by measuring the median particle size of the corresponding fractions before forming the mixture. In the particle mixture, the corresponding median particle sizes α, β and γ can be determined by the particle size distribution of the powder mixture by calculation methods. Wherein, each of the particle fractions usually has a symmetrical particle size distribution (Gaussian form) or an asymmetric particle size distribution (Gaussian form where one side of the distribution is steeper than the other side). If such distributions are superimposed in the distribution spectrum of the particle mixture, the intermediate particle size of the dominant fraction is obviously a peak, while the non-dominant fraction will appear as a peak or shoulder. Thus, the corresponding median particle size of the less dominant fraction can then be determined by simulating the superimposed particle size distribution with an assumed equal degree of symmetry.
[0017] Therefore, it is not necessary to know whether a given particle belongs to particle fraction A, B or C, since the determination of the median particle size and amount is based on the sum of all particles and the particle size distribution of the powder mixture as a whole.
[0018] The corresponding particle fractions in the powder mixture of the present invention are not limited in the material forming the fractions, i.e. the corresponding fractions can be formed by the same or different materials. However, large differences in the densities of different materials should still be avoided, because such differences can promote the separation of the corresponding materials. Therefore, preferably, the densities of the materials providing the corresponding particle fractions differ from each other by less than 50%, more preferably less than 40%, even more preferably less than 30%, and even more preferably less than 15%. In one embodiment, the corresponding particle fractions A, B and C are based on substantially the same material, in which case the densities of the materials providing the corresponding particle fractions are approximately the same. Here, "substantially" means that the composition of the corresponding fractions may have a small change, such as a combination difference of each element in the composition of at most 2% by weight and preferably at most 1% by weight (i.e. if all the amounts of the other elements are the same, a 0.5% by weight difference of Fe and a 0.5% by weight difference of Ni are 1% by weight).
[0019] In a preferred embodiment, the powder mixture of the present invention further comprises a particle fraction D having a median particle size δ greater than the median particle size β but less than the median particle size α, i.e. the median particle size δ is intermediate between the particle sizes β and α. For such a composition, it is advantageous if the particle size of the particle fraction D is 0.6-0.8 / 1, and preferably 0.65-0.76 / 1, relative to the particle size of the fraction A.
[0020] In a particularly preferred embodiment, the respective particle fractions A, B and C are based on the same material, in which case the density of the material providing the respective particle fractions is the same except for the changes caused by processing the material into powders. In another particularly preferred embodiment, the powder mixture according to the invention comprises a particle fraction D, and the particle fractions A, B, C and D have essentially the same composition. The above densities are "material densities" without any trapped gas, so the respective particle fractions may still have different bulk densities.
[0021] As indicated above, the powder mixture of the present invention is not optimized for a theoretical density of the powder mixture that is as high as possible, but is designed to provide an optimal compromise between high density and processability in additive manufacturing. Thus, the powder mixture of the present invention has a relative density of at least 50%, more preferably at least 52%, even more preferably at least 54%, and even more preferably at least 56%. This is compared to a relative density of about 45% of a conventional powder with a Gaussian particle size distribution. On the other hand, the relative density is lower than theoretically possible, with a preferred relative density of 70% or less and more preferably 63% or less.
[0022] Here, "relative density" is the bulk density or apparent density of the powder mixture divided by the skeletal density of the metal powder. Therefore, relative density is an indirect measure of the interparticle void volume and internal pore volume of a particle mixture, which can be calculated from the relative density by the term (1-relative density).
[0023] Skeletal density is the ratio of the mass of a solid material to the sum of the volume of the solid material and the closed pores (or blind pores) within the material, as determined by ASTM B 923-21. The apparent density or bulk density is determined by a suitable method, such as according to ASTM B212-17 if the solid material is a free-flowing material, and according to ASTM B417 or ASTM B329 if the solid material is a non-flowing material. A skilled practitioner can apply the appropriate standard based on his or her common sense according to the flow characteristics.
[0024] Additionally or alternatively, preferably the powder mixture has a relative adjusted bulk density of at least 50%, more preferably at least 52%, even more preferably at least 54% and even more preferably at least 56%. The relative adjusted bulk density is determined as indicated in the Examples section. On the other hand, the relative adjusted bulk density is generally lower than theoretically possible, with preferred relative densities being 75% or lower and more preferably 70% or lower.
[0025] In one embodiment, the particle mixture is based on a mixture of metals or metal alloys, such as steel alloys, nickel alloys, aluminum alloys, titanium alloys or other alloys. If the particle mixture is based on a steel alloy, preferably the powder mixture has a particle size of 4.2 to 5.0 g / cm 3 , more preferably at least 4.4 g / cm 3 and / or less than or equal to 4.9g / cm 3 , and even more preferably at least 4.6 g / cm 3 and / or less than or equal to 4.85g / cm 3 If the particle mixture is based on an aluminum alloy, the powder mixture preferably has a relative density of 1.35 to 1.9 g / cm 3, preferably at least 1.5 g / cm 3 and / or less than or equal to 1.8g / cm 3 , and more preferably at least 1.55 g / cm 3 and / or less than or equal to 1.75g / cm 3 If the particle mixture is based on a titanium alloy, the powder mixture preferably has a relative density of 2.2 to 3.1 g / cm 3 , more preferably at least 2.4 g / cm 3 and / or less than or equal to 2.9g / cm 3 , and even more preferably at least 2.5 g / cm 3 and / or less than or equal to 2.8g / cm 3 The relative density.
[0026] In another embodiment, the particle mixture is based on an organic polymer. If so, preferably the powder mixture has a particle size of 0.5 to 0.9 g / cm 3 , more preferably at least 0.55 g / cm 3 and / or less than or equal to 0.85g / cm 3 , and even more preferably at least 0.6 g / cm 3 and / or less than or equal to 0.8g / cm 3 The relative density.
[0027] Herein, the reference that "the mixture is based on" a certain material is intended to mean that at least the major volume fraction (i.e., 50% by volume or more) of the particle mixture is provided by this material. Preferably, at least 60% by volume, more preferably at least 70% by volume, and even more preferably at least 80% by volume of the particle mixture is provided by the material "the mixture is based on". In one embodiment, the mixture is based only on this material.
[0028] As noted above, the particle mixture may be based on a metal alloy, such as a steel alloy, a nickel alloy, an aluminum alloy, a titanium alloy. Possible steel alloys that may form the basis or the entire particle mixture include, for example, 316L, 18Ni300, or 17-4PH steel. Possible nickel alloys that may form the basis or the entire particle mixture include IN 718. Possible titanium alloys that may form the basis or the entire particle mixture include TiAl6V4.
[0029] In a particularly preferred embodiment, the particles in fractions A, B and C and, if present, fraction D, are steel, titanium, nickel or aluminium alloy particles, and in particular steel particles.
[0030] With regard to the organic polymers that may be contained as a substrate in the powder mixture or that may constitute part of the powder mixture, the present invention is not subject to any relevant restrictions. Examples of suitable polymers for the purposes of the present invention include polymers, copolymers or polymer blends selected in particular from the following: polyamides, polyolefins, in particular in the form of polyethylene or polypropylene, polystyrenes, polyaryletherketones (PAEK), in particular polyetherketoneketones or polyetherketones, thermoplastic polyurethanes, polyesters, polyethers, polyhydroxy acids, polylactic acid, polyphenylene sulfide, polyphenylene oxide, polyimides, polyetherimides, polycarbonates and polyether block amides (PEBA). Preferably, the polymer powder is formed from one of these polymers. Here, the term "polymer" also includes oligomers having a cyclic or annular molecular structure.
[0031] Suitable PAEK polymers and copolymers are, for example, selected from: polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyetherketone (PEK), polyetheretherketoneketone (PEEKK), polyetherketoneetherketoneketone (PEKEKK), polyaryletheretheretherketone (PEEEK) and copolymers comprising at least one of the above polymers.
[0032] In a particularly preferred embodiment, the polymer is selected from polyamides, especially in the form of polyamide-5.6, polyamide-5.10, polyamide-6, polyamide-6.6, polyamide-6.13, polyamide-11, polyamide-12, polyamide-10.12 or polyamide 12.12. Even more preferably, the polymer is selected from polyamide-11 and polyamide-12. Another particularly preferred polymer is polypropylene. Yet another particularly preferred polymer is polyether block amide (PEBA).
[0033] If the powder mixture is based on an organic polymer, the powder mixture or its individual fractions may contain additives commonly used in plastic powders for additive manufacturing, such as flow agents, anti-agglomeration agents, reflective particles and / or pigments. Suitable types of reflective particles include, for example, TiO2, which can be incorporated into plastic powders in dry form. Suitable flow agents and / or anti-agglomeration agents are, for example, carbon black or pyrolytic silica. In the case where the polymer material does not absorb light, a particularly preferred type of additive that can be used to impart absorption properties at a certain wavelength is an IR or NIR radiation absorbing material, such as the carbon black type described in WO 2020 / 099236 A1. Such materials may exist alone in a mixture with polymer-based particles, be absorbed on the surface of the particles, or be incorporated into the particles. In addition, technical polymers typically contain stabilizers (e.g., antioxidants, UV stabilizers), chain growth limiters and / or other additives for controlling polymerization reactions (e.g., acidic buffer systems), functional additives (e.g., flame retardants), and / or expected or unexpected contaminants (e.g., catalysts, compatibilizers, processing aids) from the polymerization or powderization process.
[0034] The particle size of the fraction has a great influence on the roughness of the surface produced by the additive manufacturing process from the particle mixture. For example, if the corresponding particle size is larger, the production will be faster, but the roughness of the article produced by the method will also be higher. Therefore, in order to provide a suitable compromise between production speed and surface roughness, fraction A preferably has a particle size D50 of 25 μm to 60 μm, more preferably 30 μm to 60 μm, even more preferably at least 35 μm and / or less than or equal to 52 μm, and more preferably at least 38 μm and / or less than or equal to 48 μm. In this case, the particle size is the median particle size as defined above, which is determined by laser diffraction according to ISO 13320:2020.
[0035] Particle fraction B preferably has a particle size D50 of 8 to 25 μm, and more preferably at least 10 μm and / or 20 μm or less, and even more preferably at least 12 μm and / or 17 μm or less. Particle fraction C preferably has a particle size D50 of 35 to 100 μm, more preferably 50 to 100 μm, even more preferably at least 58 μm and / or 90 μm or less, and even more preferably at least 62 μm and / or 80 μm or less. Particle fraction D, if present, preferably has a particle size D50 of 20 to 35 μm, more preferably at least 24 μm and / or 32 μm or less.
[0036] In addition to the actual particle size D50, the particle size distribution is also determined by the distribution width of the corresponding particle fraction. In the present invention, this factor is represented by "distribution width" or "span", calculated as (D90-D10) / D50. In a preferred embodiment, particle fraction A has a span of 0.3 to 1, preferably 0.4 to 1, and more preferably greater than or equal to 0.55 and / or less than or equal to 0.8. The preferred span of particle fraction B is 0.8 to 1.7, and more preferably greater than or equal to 1.0 and / or less than or equal to 1.4. For particle fraction C, the preferred distribution width is 0.2 to 0.6, more preferably 0.3 to 0.6, and even more preferably greater than or equal to 0.35 and / or less than or equal to 0.5. If particle fraction D is present, the preferred distribution width of this fraction is 0.3 to 1.0, more preferably 0.4 to 0.9, and even more preferably greater than or equal to 0.6 and / or less than or equal to 0.7.
[0037] When the powder is applied to a flat surface for subsequent processing, in order to ensure the formation of a substantially uniform powder bed, it is desirable that the corresponding particles are substantially spherical, thereby avoiding wedging between particles that can accelerate the formation of pores. Therefore, it is preferred that at least one of the particle fractions A, B and C has a sphericity of at least 0.9, in particular at least 0.93. In a particularly preferred embodiment, all particle fractions A, B and C have a sphericity of at least 0.9 and in particular at least 0.93. Here, the sphericity is the particle size x determined according to ISO 13322-2:2021 for the minimum of all the largest chords of the particle projection of the particle. c min / Particle size x, the longest Feret diameter among all Feret diameters measured for the particle Fe max In another embodiment, preferably particles A and C, or in an embodiment with particle fractions A, B, C and D, particle fractions A, D and C, have a sphericity of at least 0.9, in particular at least 0.93, whereas particle fraction A has a more irregular shape, for example having a sphericity of less than 0.9 and in particular less than 0.7.
[0038] Finally, the relative density provided by the powder mixture is also affected by the ratio of the corresponding particle fractions. Therefore, a powder mixture preferably used in the present invention comprises 10 to 20 parts by weight of particle fraction B, 50 to 70 parts by weight of particle fraction A and 10 to 40 parts by weight of particle fraction C, based on the total weight of the mixture. In another preferred powder mixture, particle fraction B accounts for 10 to 25 parts by weight, particle fraction A accounts for 4 to 15 parts by weight and particle fraction C accounts for 55 to 80 parts by weight, based on the total weight of the mixture. In another preferred powder mixture, particle fraction B accounts for 2 to 20 parts by weight, particle fraction A accounts for 10 to 25 parts by weight and particle fraction C accounts for 55 to 80 parts by weight, based on the total weight of the mixture; for such a powder mixture, it is preferred that the median particle size of its particle fractions B, A and C is related to each other by 0.2-0.5 / 1 / 1.2-1.5. If the powder mixture according to the invention comprises a powder fraction D, the corresponding weight ratios B / D / A / C are preferably 5-15 / 10-25 / 50-70 / 10-20 parts by weight.
[0039] In a second aspect, the present invention relates to a method for preparing a powder mixture, preferably a powder mixture as described above, wherein the method comprises: providing a particle fraction A having a median particle size α, a particle fraction B having a median particle size β less than the median particle size α, and a particle fraction C having a median particle size γ greater than the median particle size α, wherein the particle sizes of the particle fractions B, A and C are related to each other by 0.2-0.5:1:1.2-2, and mixing the particle fractions A, B and C to provide a powder mixture. Preferably, the particle fractions in the above method have substantially the same composition. In one embodiment, the powder mixture further comprises the particle fraction D as described above.
[0040] Mixing can be achieved by any conventional means by which powder mixtures can be prepared, and will most conveniently be accomplished by dry mixing of the corresponding particle fractions. These in turn can be prepared by means commonly used for powder production, such as gas and plasma atomization to produce metal and metal alloy powders, or by cryogenic grinding with optional subsequent rounding treatment.
[0041] In a third aspect, the present invention relates to a method for manufacturing a three-dimensional object, comprising providing a powder mixture as defined above, wherein preferably the powder mixture is prepared according to the method described above, and preparing the object by applying the mixture layer by layer and selectively consolidating the mixture, in particular by applying electromagnetic radiation at positions in each layer corresponding to the cross-section of the object in that layer, wherein the positions are scanned in at least one interaction zone, in particular in the radiation interaction zone of the energy beam.
[0042] The energy beam provides enough energy to melt the powder mixture in the irradiation zone. As will be appreciated by a skilled practitioner, the irradiated powder depends on the material of the powder mixture (more energy is required to melt metals or metal alloys than organic polymers). In most cases, the energy beam will be an electron beam or an electromagnetic radiation beam. In a particularly preferred embodiment, the electromagnetic radiation beam is provided by a laser, which can easily provide the required amount of power. If less power is required, such as in the case of processing polymer powders, a diode laser, an array of diode lasers, or a surface emitter (VCSEL or Philips-VCSEL) can also be used as an energy source or energy beam emission source.
[0043] As indicated above, the thickness of the applied layer has an influence on the surface roughness of the produced three-dimensional object. Therefore, the thickness of the layer is usually adjusted to provide a compromise between production speed and surface roughness. Therefore, in a preferred embodiment, the corresponding individual layers are applied with a thickness of 10 μm or more, in particular 20 μm or more, and more preferably 30 μm or more. In order to ensure that the roughness is not too high and a substantially uniform melting (which may be impaired if the layer to be melted becomes thicker), the thickness of the layer is preferably 160 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and even more preferably 60 μm or less.
[0044] The process is preferably carried out using a volume ratio of 5 to 12, and more preferably at least 6.5 and / or less than or equal to 10.5, and even more preferably 9.8 or less.
[0045] Suitable methods for processing the powder mixtures indicated above include, but are not limited to: direct metal laser sintering (DMLS) and direct metal laser melting (DMLM) for powder mixtures based on metals or metal alloys; and selective laser sintering (SLS), selective laser melting (SLM) for powder mixtures based on organic polymers. Still further, three-dimensional objects based on organic polymers can be prepared by multi-jet modeling (wherein a liquid photosensitive plastic material containing the additives conferring biodegradability indicated above is applied to a platform by a print head and cured by a radiation source incorporated into the print head), or other methods involving the continuous provision of powder layers as part of the manufacturing process.
[0046] After the three-dimensional object has been produced, it may be subjected to conventional processing steps, including heat treatments to adjust the mechanical properties of objects made of metals or metal alloys, or chamfering processes to smooth the surface of the object, such as grinding, etching or other surface abrasive processes.
[0047] In a fourth aspect, the present invention relates to a three-dimensional object prepared according to the method described above, i.e., a method for preparing a three-dimensional object by selectively solidifying a powder mixture layer by layer at positions in the corresponding layers corresponding to the cross-section of the object by electromagnetic and / or particle radiation, wherein the powder mixture is a powder mixture for manufacturing a three-dimensional object by additive manufacturing, wherein the powder mixture comprises a particle fraction A having a median particle size α, a particle fraction B having a median particle size β smaller than the median particle size α, and a particle fraction C having a median particle size γ larger than the median particle size α, wherein the particle sizes of the particle fractions B, A and C are related to each other at 0.2-0.5:1:1.2-2.
[0048] In one embodiment, the three-dimensional object is a three-dimensional object having a defect percentage of 0.050% or less, preferably 0.020% or less, more preferably 0.015% or less, and even more preferably 0.010% or less.
[0049] In a fifth aspect, the present invention relates to the use of a powder mixture as defined above for reducing the number of defects in a three-dimensional object produced from the powder mixture by an additive manufacturing process. Here, "defects" include porosity originating from fusion defects that trap ambient gases or poorly melted areas, as assessed by image analysis of a cross section of the object. For the purposes of the present invention, the number of defects is indicated as a percentage of the "defective" area relative to the entire area studied.
[0050] In a sixth aspect, the present invention relates to an apparatus for implementing the method for producing a three-dimensional object as described above, wherein the apparatus comprises: an irradiation unit emitting electromagnetic or particle radiation, preferably a laser sintering or laser melting device 20, a processing chamber 3 having an open container 5 with a container wall 6, a support 10 in the processing chamber 3, wherein the open container 5 and the support 10 are movable relative to each other in the vertical direction, a storage container 14 and a recoater 16 movable in the horizontal direction, and wherein the storage container 14 is at least partially filled with the powder mixture defined above.
[0051] Other features and embodiments of the present invention are provided by considering the following Figure 1 In the following description of exemplary embodiments.
[0052] Figure 1 The device represented in is a laser sintering or laser melting apparatus 1 for producing a three-dimensional object 2. The apparatus 1 comprises a processing chamber 3 having a chamber wall 4. A container 5 which is open at the top and has a container wall 6 is arranged in the processing chamber 3. The opening at the top of the container 5 delimits a working surface 7. The part of the working surface 7 which is located within the opening of the container 5 and can be used to build the object 2 is called the building area 8. In the container 5, a support 10 is arranged, which is movable in a vertical direction V, and to which is attached a substrate 11 which closes the container 5 towards the bottom and thus forms the base of the container 5. The substrate 11 can be a plate formed separately from the support 10 and fastened to the support 10, or can be formed so as to constitute an integral part with the support 10. A building platform 12 on which the object 2 is built can also be attached to the substrate 11. However, the object 2 can also be built on the substrate 11, which then acts as a building platform itself.
[0053] exist Figure 1, the object 2 to be manufactured is shown in an intermediate state. It consists of a plurality of solidified layers and is surrounded by still unsolidified building material 13. In addition, the apparatus 1 comprises a storage container 14 for a building material 15 in powder form, which can be solidified by electromagnetic radiation, such as laser and / or particle radiation, such as electron beam. The apparatus 1 also comprises a recoater 16, which is movable in a horizontal direction H for applying layers of building material 15 in the building area 8. Optionally, a radiation heater 17, such as an infrared heater, for heating the applied building material 15 can be arranged in the processing chamber.
[0054] also, Figure 1 The device in the embodiment includes an irradiation device 20 having a laser 21, which generates a laser beam 22 which is deflected by a deflection device 23 and focused on the working surface 7 via an incident window 25 by a focusing device 24. The incident window 25 is arranged in the top surface of the processing chamber 3 and the chamber wall 4.
[0055] also, Figure 1 The apparatus in the apparatus 1 comprises a control unit 29, by which the individual components of the apparatus 1 are controlled in a coordinated manner to carry out the method for manufacturing a three-dimensional object. The control unit 29 may comprise a CPU, the operation of which is controlled by a computer program (software). During operation of the apparatus 1, the following steps are repeated: for each layer, the support 10 is lowered to a height preferably corresponding to the desired thickness of the layer of the building material 15. The recoater 16 is moved to the storage container 14, from which it receives a sufficient amount of building material 15 to apply at least one layer. The recoater 16 then moves over the building area 8 and applies a thin layer of the building material 15 in powder form on the substrate 11 or on the building platform 12 or on the previously applied layer. The layer is applied at least across the cross section of the object 2, preferably across the entire building area 8. Optionally, the building material 15 is heated to the operating temperature by at least one radiant heater 17. Then, the cross section of the object 2 to be manufactured is scanned with a laser beam 22 to selectively cure the area of the applied layer. These steps are carried out until the object 2 is completed. The object 2 can then be removed from the container 5.
[0056] According to the present invention, a powder mixture is used as a building material 15. The powder mixture comprises a particle fraction A having a median particle size α, a particle fraction B having a median particle size β smaller than the median particle size α, and a particle fraction C having a median particle size γ larger than the median particle size α, wherein the particle sizes of the particle fractions B, A and C are related to each other by 0.2-0.5 / 1 / 1.2-2.
[0057] According to the embodiments described below, when the powder mixture is based on a metal or a metal alloy, the powder mixture is processed, for example, by a direct metal laser sintering (DMLS) method. In selective laser sintering or selective laser melting, small portions of the entire volume of powder required to manufacture the object are heated simultaneously to a temperature that allows these portions to sinter and / or melt. This way of manufacturing an object can generally be characterized as a continuous and / or often gradual process at a microscopic level, whereby the object is obtained by multiple heating cycles of small powder volumes. The solidification of these small powder portions is carried out selectively, i.e. at selected locations of the powder reservoir corresponding to the portion of the object to be manufactured. As in selective laser sintering or selective laser melting, the process of solidification is generally carried out layer by layer, the solidified powder in each layer being identical to the cross-section of the object to be constructed. Due to the small volume or mass of the powder, it is measured in layers of, for example, 1 mm 3 The material solidifies in a given time span of one second or less, and due to the conditions in the processing chamber of such additive manufacturing machines, which can facilitate rapid cooling to below the critical temperature, the material generally solidifies quickly after heating.
[0058] In conventional sintering and casting methods, parts of the same building material are heated to the required temperature at the same time. The entire part of the material required to produce the object is poured into the mold in liquid form. Therefore, compared to selective laser sintering or selective laser melting, the volume of building material is kept at a temperature level higher than that required for melting or sintering for a much longer time. The large volume of hot material leads to a low cooling rate and a slow solidification process of the building material after heating. In other words, selective laser sintering or selective laser melting can be distinguished from conventional sintering and casting methods by: processing smaller volumes of building materials, faster thermal cycles, and less need for building materials with high resistance to heating to avoid premature solidification of the material. These can be counted as the reason why the amount of energy introduced into the building material to reach the required temperature in selective laser sintering or selective laser melting can be more accurately controlled. These conditions allow the upper limit of the energy input of the powder part to be processed to be set, which determines the temperature generated in the powder part, more precisely, it is lower than the conventional sintering or casting method and is closer to the melting point of the corresponding material.
[0059] Objects produced from powder mixtures according to the present invention may show changes in various mechanical properties, but most notably show reduced defects relative to objects prepared from conventional AM powders.
[0060] The present invention will be further described below by some examples, however, the examples are not to be construed as limiting the present invention in any way.
[0061] Example 1: Preparation of a powder mixture according to the invention
[0062] In a mixer, a first particle fraction B of 316L steel having a D50 of 14.3 μm, a second particle fraction A of 316L steel having a D50 of 42.6 μm, and a third particle fraction C of 316L steel having a D50 of 70.8 μm were mixed to provide a powder mixture. In the mixture, the first particle fraction had a span of 1.14, the second particle fraction had a span of 0.62, and the third particle fraction had a span of 0.42. The amounts of the corresponding particle fractions were 15 / 70 / 15, respectively. The resulting powder had a particle size of 4.94 g / cm 3 The relative density of the powder mixture is Figure 2 Shown in.
[0063] In comparison, conventional 316L steel powder with a median particle size of about 35 μm has a particle size of 3.9 g / cm 3 Therefore, the powder of the present invention has a relative density that is about 25% higher than that of conventional powder.
[0064] The composition and apparent density of other powder mixtures according to the invention are given in Table 1 below:
[0065]
[0066] Example 2: Processing of the powder mixture of the invention
[0067] In an EOS-M290 machine, test specimens of inventive and conventional 316L steel powder were prepared using varying volume ratios (VR). In these test bodies, cross sections were prepared and evaluated for defects by image analysis.
[0068] The results of these tests are given in Table 2 below:
[0069] <![CDATA[VR[mm 3 / s]]]> Comparative 316 powder 316 powder of the present invention defect% defect% Total defects defect% Total defects 6.8 0.021 499 0.007 204 7.8 0.060 1257 0.023 758 8.0 0.024 602 0.012 747 8.2 0.078 2220 0.031 1110 8.4 0.063 1199 0.024 849 9.0 0.142 2028 0.077 1643 9.2 0.075 1538 0.032 733 9.5 0.314 3859 0.208 3109 9.6 0.050 1289 0.020 836 10.1 0.399 3087 0.265 2104 average 0.123 1758 0.070 1209
[0070] The table above shows that by using the powder mixture of the present invention, the percentage and total number of defects can be reduced by about 75% (defect %) and 50% (total defects) on average.
[0071] Example 3: Reusability of the powder mixture of the present invention
[0072] The particle size distribution and apparent density of the powder mixture of 316L steel remaining from the production of the test specimens by processing in an EOS M290 machine were investigated. The corresponding D10, D50 and D90 particle sizes were determined according to ISO 13322:2020 after one, five and nine processings of the corresponding material without melting. The results of these tests are given in the following Table 3:
[0073] After 1 processing After 5 processing After 9 processing D10 14.1 17.5 17.8 D50 39.2 40.7 40.7 D90 57.7 60.3 61.6 Apparent density 4.7 4.7 4.7
[0074] It is evident from the above table that when the granular powders are processed so that they can be reused without further conditioning, there is minimal change in the corresponding D10, D50 and D90.
[0075] Embodiment 4:
[0076] Different powder mixtures according to the invention were prepared from 316L steel powder. The compositions and relative adjusted bulk densities are provided in the following Tables 4 to 6:
[0077] Table 4
[0078]
[0079] (x / A is B / A for particle fraction B, A / A for particle fraction A and C / A for particle fraction C)
[0080] Table 5
[0081]
[0082] Table 6
[0083]
[0084] In the above table, the adjusted bulk density was determined as described in A. Lüddecke et al., Materials and Design 202 (2021), 109536. The relative adjusted density is calculated therefrom as adjusted bulk density / true metal (or metal alloy) density×100%.
[0085] Example 5
[0086] A set of test specimens was prepared using standard 316L steel powder (powder size 20 to 65 μm, monomodal particle size distribution) and corresponding powders of this material according to the specifications in Tables 4 and 6 above. The samples were prepared using a laser speed of 850 mm / s, a laser power of 320 W and a window distance of 0.16 mm. After preparation, the defect percentage (D-%) and the number of defects >100 μm and >150 μm of the corresponding samples were studied.
[0087] The results of these tests are given in Table 7 below:
[0088] Table 7
[0089] D-% Defects >100μm Defects >150μm Standard 316L 0.823% 92 22 According to Table 4, 316L 0.533% 55 7 According to Table 6, 316L 0.581% 61 9
[0090] As can be seen from this comparison, the powder mixture according to the invention allows the production of objects with fewer defects. Since defects have a great influence on the mechanical properties of an object, it can be expected that under the same production conditions, the powder mixture of the invention allows the production of objects with improved mechanical properties.
Claims
1. A powder mixture for additive manufacturing, wherein the powder mixture comprises a particle fraction A having a median particle size α, a particle fraction B having a median particle size β smaller than the median particle size α, and a particle fraction C having a median particle size γ larger than the median particle size α, wherein the particle sizes of the particle fraction B, the particle fraction A, and the particle fraction C are related to each other by 0.2-0.5 / 1 / 1.2-2.
2. The powder mixture according to claim 1, wherein the median particle sizes of particle fraction B, particle fraction A and particle fraction C are related to each other by 0.25-0.4 / 1 / 1.4-1.
8.
3. A powder mixture according to claim 1 or 2, further comprising a particle fraction D having a median particle size δ greater than the median particle size β but less than the median particle size α, and wherein the particle size of the particle fraction D is related to the particle size of the fraction A by 0.6-0.8 / 1 and preferably 0.65-0.76 / 1.
4. A powder mixture according to any one of claims 1 to 3, wherein the particle fraction A, particle fraction B and particle fraction C have substantially the same composition, and preferably wherein the particle fraction A, particle fraction B, particle fraction C and particle fraction D have substantially the same composition.
5. Powder mix according to any of the preceding claims, wherein the powder mix has a relative density and / or relative adjusted bulk density of at least 50%, and preferably at least 54% and / or below 70%.
6. A powder mixture according to any one of the preceding claims, wherein the powder mixture has a viscosity of 4.2 to 5.0 g / cm 3 , preferably at least 4.4 g / cm 3 and / or less than or equal to 4.9g / cm 3 , and more preferably at least 4.6 g / cm 3 and / or less than or equal to 4.85g / cm 3 The apparent density of .
7. A powder mixture according to any one of the preceding claims, wherein the particle fraction A has a particle size D50 of 25 to 60 μm, preferably 30 to 60 μm, more preferably at least 35 μm and / or less than or equal to 52 μm, and even more preferably at least 38 μm and / or less than or equal to 48 μm.
8. The powder mixture according to any one of the preceding claims, wherein the particle fraction B has a particle size D50 of 8 to 25 μm, and preferably at least 10 μm and / or ≤ 20 μm, and more preferably at least 12 μm and / or ≤ 17 μm.
9. A powder mixture according to any one of the preceding claims, wherein the particle fraction C has a particle size D50 of 35 to 100 μm, preferably 50 to 100 μm, more preferably at least 58 μm and / or less than or equal to 90 μm, and even more preferably at least 62 μm and / or less than or equal to 80 μm.
10. A powder mixture according to any of the preceding claims, wherein the particle fraction A has a distribution width indicated by a span of 0.3 to 1 and preferably 0.55 to 0.8, and / or the particle fraction B has a distribution width indicated by a span of 0.8 to 1.7 and preferably 1.0 to 1.4, and / or the particle fraction C has a distribution width indicated by a span of 0.2 to 0.6 and preferably 0.35 to 0.
5.
11. A powder mixture according to any of the preceding claims, wherein the particle fraction A and / or the particle fraction B and / or particle fraction C have a sphericity of at least 0.9, in particular at least 0.93, preferably wherein all particle fractions have a sphericity of at least 0.9, preferably wherein the particle fraction A and particle fraction C have a sphericity of at least 0.9 and wherein the particle fraction B is irregular.
12. A powder mixture according to any one of the preceding claims, wherein the particle fraction B accounts for 10 to 20 weight parts, the particle fraction A accounts for 50 to 70 weight parts and the particle fraction C accounts for 10 to 40 weight parts, based on the total weight of the mixture; or wherein the particle fraction B accounts for 2 to 20 weight parts, the particle fraction A accounts for 10 to 25 weight parts and the particle fraction C accounts for 55 to 80 weight parts, based on the total weight of the mixture.
13. The powder mixture according to any one of the preceding claims, wherein the particles in fraction A, particle fraction B and particle fraction C are steel, titanium, copper, chromium, zirconium, nickel or aluminium alloy particles, preferably steel particles.
14. A method for preparing a powder mixture, preferably a powder mixture as described in any one of claims 1 to 13, comprising providing a particle fraction A having a median particle size α, a particle fraction B having a median particle size β smaller than the median particle size α, and a particle fraction C having a median particle size γ larger than the median particle size α, wherein the particle sizes of the particle fraction B, the particle fraction A and the particle fraction C are related to each other at 0.2-0.5:1:1.2-2, and mixing the particle fraction A, the particle fraction B and the particle fraction C to provide a powder mixture.
15. A method for manufacturing a three-dimensional object, comprising providing a powder mixture as defined in any one of claims 1 to 13, preferably a powder mixture prepared according to the method of claim 14, and preparing the object by applying the mixture layer by layer and selectively consolidating the mixture, specifically by applying electromagnetic radiation at positions in each layer, the positions corresponding to the cross-section of the object in the layer, wherein the positions are scanned in at least one interaction zone, specifically in the radiation interaction zone of the energy beam.
16. The method according to claim 15, wherein the individual layers are applied with a thickness of 10 μm or more, preferably 20 μm or more and more preferably 30 μm or more and / or 160 μm or less, preferably 100 μm or less and more preferably 80 μm or less.
17. A three-dimensional object produced according to the method of claim 15 or 16.
18. Use of a powder mixture according to any one of claims 1 to 13 for reducing the number of defects in a three-dimensional object produced from the powder mixture by an additive manufacturing process.
19. An apparatus for implementing the method according to claim 15 or 16, wherein the apparatus comprises: An irradiation unit for emitting electromagnetic or particle radiation, preferably a laser sintering or laser melting device (20), a processing chamber (3) having an open container (5) with a container wall (6), a support (10) in the processing chamber (3), wherein the open container (5) and the support (10) are movable relative to each other in the vertical direction, a storage container (14) and a recoater (16) movable in the horizontal direction, and wherein the storage container (14) is at least partially filled with a powder mixture according to any one of claims 1 to 13.