Core material, skin-core structure, aircraft propeller, aircraft floor panel, rocket fairing, and rocket interstage part

By using discontinuous reinforced fiber sheets and skins of fiber-reinforced composite materials, the problem of poor fiber dispersion in the manufacturing process of aramid honeycombs is solved, and core materials and skins with lightweight and high mechanical properties are achieved - The core structure improves the stability and performance of the manufacturing process.

CN118765231APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380023691.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-03-03
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing aramid honeycombs have problems with poor fiber dispersion, inconsistent paper density, poor water retention and water drainage during the manufacturing process, resulting in poor operability and changes in mechanical properties over time.

Method used

A core material composed of a sheet of discontinuous reinforcing fibers dispersed in the form of single fibers is used, combined with a skin material of fiber-reinforced composite material, and a honeycomb structure is manufactured by the stretching method or the corrugation method to ensure uniform dispersion of fibers and high strength.

Benefits of technology

The core material and skin-core structure achieve lightweight and mechanical properties, improve the texture and strength of the base material, solve the problem of fiber dispersion and operability, and enhance the overall performance of the honeycomb structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765231A_ABST
    Figure CN118765231A_ABST
Patent Text Reader

Abstract

Provided is a core material which can be manufactured smoothly by improving the texture and strength of a base material, and which has excellent strength and light weight. The present invention is a core material having a structure comprising an aggregate of hollow columnar cells partitioned by cell walls containing a sheet in which discontinuous reinforcing fibers (Cf) are dispersed in the form of single fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a core material having light weight and mechanical properties and a skin-core structure using the same. Background Art

[0002] The skin-core structure composed of a core material having a structure composed of an aggregate of hollow columnar units divided by unit walls and a skin material is widely used in structures such as aircraft and ships or building materials due to its excellent mechanical properties such as light weight and high rigidity. Such core materials include aluminum honeycomb cores composed of aluminum foil, FRP honeycomb cores composed of reinforcing fibers and matrix resins, etc. Among them, for flying objects such as aircraft that require strong lightweight, aramid honeycomb cores made by impregnating phenolic resin in non-woven fabrics of aramid fibers are mainly used in view of light weight and mechanical properties.

[0003] The aramid sheet as the base material of the aramid honeycomb described in Patent Document 1 contains or is compounded with 0% to 50% by weight of a binder and 50% to 100% by weight of para-aramid fibers. In the aramid honeycomb that is then post-treated to attach and impregnate a reinforcing resin, the para-aramid fibers are finally contained at a weight ratio of 20% to 80%. For this aramid honeycomb, there is a difficulty in that the texture of the aramid sheet is not good. That is, a large amount of fibers, that is, para-aramid fibers with a content of more than 50%, tend to expand in volume during handling. Therefore, when the aramid sheet is used for papermaking, it is difficult to uniformly stir it with papermaking liquid such as water, and it is difficult to disperse it on a filter for papermaking. Therefore, the para-aramid fibers of the aramid sheet obtained by papermaking have poor dispersibility, inconsistent paper density, deviations, etc., and the texture is poor. In addition, the water retention and water filtration are poor, and the fixation of the adhesive mixed into the papermaking liquid such as water during papermaking is reduced. Moreover, since the adhesive is not fixed and flows down after being compounded on the para-aramid fiber, there are also difficulties in the paper strength of the aramid sheet. Therefore, wrinkles are generated in the part with more para-aramid fiber and the part with less para-aramid fiber. When manufacturing aramid honeycombs, sometimes the operability is poor, large pinholes are generated, and there are problems such as adhesive shedding, which also hinder the manufacture of aramid honeycombs. Moreover, since aramid fibers are easy to absorb moisture, there is sometimes a problem that the mechanical properties change over time.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 4-226745 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In view of such actual conditions, an object of the present invention is to provide a core material which can be smoothly manufactured by improving the texture and strength of a base material and has excellent strength and lightness.

[0009] Solution

[0010] In order to solve the above-mentioned problems, the present invention provides a core material having a structure composed of an aggregate of hollow columnar cells partitioned by cell walls containing a sheet in which discontinuous reinforcing fibers Cf are dispersed in the form of single fibers.

[0011] The present invention is also a skin-core structure in which a skin material made of a fiber-reinforced composite material is joined to the core opening surface of the core material.

[0012] Effects of the Invention

[0013] According to the present invention, a core material and a skin-core structure having lightness and good mechanical properties can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic diagram showing an example of the dispersion state of the reinforcing fibers in the core material sheet of the present invention.

[0015] Figure 2 This is a schematic diagram showing an example of a burning jig for measuring the two-dimensional orientation angle of a sheet.

[0016] Figure 3 This is a schematic diagram showing an example of an apparatus for producing a papermaking base material.

[0017] Figure 4 It is a schematic diagram showing one embodiment of the skin-core structure of the present invention.

[0018] Figure 5 This is a schematic diagram showing an example of the average fiber orientation angle in the in-plane direction of the cell wall surface of the reinforcing fiber (Cf) of the present invention.

[0019] Figure 6 This is a schematic diagram showing a state in which a part of the discontinuous fibers (Cf) included in the cell walls of the core material has entered the skin material. DETAILED DESCRIPTION

[0020] <Core material>

[0021] The core material of the present invention is described below with reference to the accompanying drawings as appropriate, but the present invention is not limited to these drawings. However, as those skilled in the art will readily appreciate, the description of the embodiments described in the accompanying drawings can also serve to illustrate the core material of the present invention as a higher concept.

[0022] The core material of the present invention has a structure composed of an aggregate of hollow columnar units formed by cell wall division. The unit shape of the core material is not particularly limited, and can be a polygon such as a triangle, a quadrilateral, a hexagon, a circle or an ellipse, etc. From the viewpoint of impact resistance, a regular hexagonal honeycomb core is preferred. In the case where the shape of the unit is a regular hexagon, the length of one side of the regular hexagon is generally 3mm to 20mm, but from the viewpoint of the contact point with the adhesive, it is preferred to use a unit with a length of 3mm to 10mm on one side of the regular hexagon, and more preferably a unit of 3mm to 7mm. In addition, a combination of unit shapes composed of a plurality of polygons (a cross-sectional shape perpendicular to the axial direction of the columnar unit) can suppress the characteristic deviation in the core material, and at the same time make the opening surface a curved surface shape or a sphere, so it is preferred. As a combination of polygons, for example, a truncated icosahedron formed by combining a pentagon and a hexagon, a curved surface shape using a part thereof, etc. can be cited.

[0023] The core material of the present invention can be made with the sheet material described later as the base material, for example, by the well-known spreading method or corrugation method. In the spreading method, a bonding material such as an adhesive is applied to the sheet material in strips, and after overlapping multiple sheets with the applied bonding material staggered by half a pitch, they are bonded by heating and pressurizing, and stretched along the overlapping direction to obtain a core material. In the corrugation method, the sheet material is first bent into a corrugated plate, and multiple corrugated plates are staggered by half a wave pitch (pitch) of the wave, and each valley and top are stacked into a block with a bonding material such as an adhesive sandwiched therebetween, and then heated and pressurized to bond them, thereby obtaining a core material.

[0024] The cell wall of the core material is composed of a sheet formed by impregnating a resin (Cr) in a reinforcing fiber substrate in which discontinuous reinforcing fibers (Cf) are dispersed in a single fiber form. It is preferred that all cell walls constituting the core material are composed of such a sheet, but as long as at least a portion of the cell walls are composed of such a sheet, the effect of the present invention can be obtained. The reinforcing fiber substrate of the cell wall refers to a precursor in which the reinforcing fibers are processed into a sheet, a cloth or a mesh, as long as there is a gap impregnated with resin between the reinforcing fibers, and there is no particular restriction on its form or shape. For example, the reinforcing fibers can be mixed with organic fibers, organic compounds or inorganic compounds, and the reinforcing fibers can be filled with other components, and the reinforcing fibers can also be bonded with resin components. From the perspective of easily realizing the two-dimensional orientation of the reinforcing fibers of the present invention, it can be illustrated that the substrate in which the non-woven fabric morphology obtained by a dry method or a wet method is fully opened and the reinforcing fibers are filled with organic compounds is a preferred shape.

[0025] In addition, the reinforcing fiber substrate used in the present invention preferably has sufficient voids to be impregnated with the resin component as the matrix, so it is preferable to ensure the air permeability of the reinforcing fiber substrate. The air permeability can be measured, for example, by the Gurley tester method based on JIS P 8117 (2009) or the Frazier method based on ASTM D 737 (2008). Among them, in order to evaluate a material with better air permeability, it is preferable to use the air volume (cm2) measured by the Frazier method based on ASTM D737. 3 / cm 2 ·s), the preferred air volume is 50 or more, more preferably 70 or more, and particularly preferably 100 or more. The upper limit of the air volume is not particularly limited, but generally 1000 or less can be exemplified.

[0026] As the reinforcing fiber for reinforcing the fiber substrate, there is no particular restriction, for example, carbon fiber, glass fiber, aramid fiber, alumina fiber, silicon carbide fiber, boron fiber, metal fiber, natural fiber, mineral fiber, etc. can be used, and they can be used 1 or in combination of 2 or more. From the viewpoint of improving the economy of the obtained molded product, glass fiber can be preferably used, especially from the balance of mechanical properties and economy, carbon fiber and glass fiber are preferably used in combination. Furthermore, from the viewpoint of improving the impact absorbency and shapeability of the obtained molded product, aramid fiber can be preferably used, especially from the balance of mechanical properties and impact absorbency, carbon fiber and aramid fiber are preferably used in combination. In addition, from the viewpoint of improving the conductivity of the obtained molded product, reinforcing fibers covering metals such as nickel, copper, and ytterbium can also be used. Among them, from the viewpoint of no water absorption problem, and high specific strength and specific rigidity, lightweight effect, it is particularly preferred to use carbon fibers such as PAN system, asphalt system, and rayon system.

[0027] The carbon fiber used in the present invention preferably has a tensile modulus of 200 to 600 GPa. The tensile modulus of carbon fiber is affected by the crystallinity of the graphite structure constituting the carbon fiber. The higher the crystallinity, the higher the elastic modulus. In addition, the higher the crystallinity, the higher the conductivity. If within this range, the conductivity, rigidity, and strength of the sheet are all balanced at a high level, so it is preferred. A more preferred elastic modulus is in the range of 230 to 400 GPa, and more preferably in the range of 260 to 370 GPa. Here, the tensile modulus of the reinforcing fiber is a value measured according to JIS R7601-2006. As commercially available products of carbon fiber, "トレカ (registered trademark)" T800S-24K, "トレカ (registered trademark)" T300-3K, "トレカ (registered trademark)" M55J-6K, and "トレカ (registered trademark)" T700S-12K (the above are made by Toray Industries, Ltd.) and the like can be cited.

[0028] As the fiber length of the reinforcing fiber constituting the reinforcing fiber substrate, it is important to be composed of 0 to 50% by mass of reinforcing fibers with a fiber length greater than 10 mm, 50 to 100% by mass of reinforcing fibers with a fiber length of 2 to 10 mm, and 0 to 50% by mass of reinforcing fibers with a fiber length less than 2 mm. If the reinforcing fiber greater than 10 mm is greater than 50% by mass, the thickness expansion in the lamination process or the molding process becomes larger, which sometimes impairs the operability. In addition, when the reinforcing fiber less than 2 mm is greater than 50% by mass, not only the mechanical properties of the sheet and the core material obtained are sometimes reduced, but also the sufficient strength of the sheet material is sometimes not ensured, which impairs the formability of the core material. From these viewpoints, it is preferred that the reinforcing fiber with a fiber length of 3 to 8 mm is 80 to 100% by mass, and it is more preferred that the distribution of the fiber length has at least 2 peaks, one peak in the range of the fiber length of 5 to 10 mm, and the other peak in the range of 2 to 5 mm. By making the distribution of fiber length within a more preferred range, it is possible to use reinforcing fibers that ensure mechanical properties and reinforcing fibers that ensure the operability of the sheet in the core material molding process, and it is easy to take both properties into account. In addition, the weight ratio of the reinforcing fibers here represents the ratio of the number average fiber length when the reinforcing fibers are set to 100%.

[0029] As a method for measuring the fiber length of the reinforcing fiber, there are methods such as directly taking out the reinforcing fiber from the reinforcing fiber substrate, or using a solvent that only dissolves the resin of the sheet to dissolve it, and filtering out the remaining reinforcing fibers, and measuring by microscopic observation (dissolution method). In the absence of a solvent for dissolving the resin, there is a method (burning method) in which only the resin is burned within a temperature range where the reinforcing fibers are not oxidatively reduced, the reinforcing fibers are classified, and the reinforcing fibers are measured by microscopic observation. In the measurement, 400 reinforcing fibers can be randomly selected, and their lengths can be measured to 1 μm units using an optical microscope to measure the fiber length and its ratio. In addition, when comparing the method of directly taking out the reinforcing fibers from the reinforcing fiber substrate with the method of taking out the reinforcing fibers from the prepreg by burning or dissolving, by appropriately selecting the conditions, the results obtained will not produce special differences.

[0030] The orientation state of the reinforcing fibers can be represented by a two-dimensional orientation angle. Generally speaking, there are many cases where the reinforcing fibers are bundled in the reinforcing fiber substrate, so it is difficult to ensure isotropy as a sheet, and the resin impregnation in the bundle is insufficient, which sometimes becomes the reason for the reduction of the strength of the core material. Even if the reinforcing fiber bundle is dispersed as a single filament, if the single filaments of the reinforcing fibers are parallel to each other, the same result will be obtained. Furthermore, excessive fiber orientation in the thickness direction becomes the reason for the thickness expansion of the sheet, which sometimes significantly impairs the operability and core material formability.

[0031] The two-dimensional orientation angle formed by one reinforcing fiber single thread and another reinforcing fiber single thread crossing the reinforcing fiber single thread will be described using the drawings. Figure 1 It is an example of a sheet material, and is a schematic diagram showing the dispersion state of the reinforcing fibers when only the reinforcing fibers are observed from a direction perpendicular to the cell wall. Focus on the reinforcing fiber monofilament 1, which crosses with the reinforcing fiber monofilaments 2 to 7. Here, the so-called crossing refers to the state in which the reinforcing fiber monofilament of interest and other reinforcing fiber monofilaments are observed to cross in the two-dimensional plane of observation. Here, in the actual sheet material, the reinforcing fiber 1 and the reinforcing fibers 2 to 7 are not necessarily in contact. The two-dimensional orientation angle is defined as the angle θ of 0° or more and 90° or less of the two angles formed by the two intersecting reinforcing fiber monofilaments.

[0032] Specifically, there is no particular limitation on the method for measuring the two-dimensional orientation angle from a sheet or core material. For example, a method for observing the orientation of the reinforcing fibers from the surface of a sample cut from a sheet or core material can be exemplified. In this case, by grinding the surface of the sample to expose the fibers, it is easier to observe the reinforcing fibers, so it is preferred. In addition, a method for observing the orientation of the reinforcing fibers using transmitted light for a sample cut from a sheet or core material can be exemplified. In this case, by cutting the sample into thin slices, it is easier to observe the reinforcing fibers, so it is preferred. In addition, a method for taking an orientation image of the reinforcing fibers by performing X-ray CT penetration observation on a sample cut from a sheet or core material can also be exemplified. In the case of reinforcing fibers with high X-ray transmittance, if fibers for tracers are mixed in the reinforcing fibers, or if tracer agents are applied to the reinforcing fibers, it is easier to observe the reinforcing fibers, so it is preferred.

[0033] In addition, when it is difficult to measure by the above method, a method of observing the orientation of the reinforcing fibers after removing the resin in a manner that does not destroy the structure of the reinforcing fibers can be exemplified. Figure 2 As shown in (a), a cell wall or sheet 10 as a sample can be sandwiched between two stainless steel meshes 9, the sample can be fixed with screws or the like so that it does not move, and then the resin component can be burned off and the obtained reinforcing fiber substrate 11 ( Figure 2 b) to determine.

[0034] The two-dimensional orientation angle of the present invention is measured according to the following steps I and II.

[0035] I. Measure and compare with a randomly selected reinforcing fiber monofilament (e.g. Figure 1 All reinforcing fiber monofilaments (e.g., Figure 1 The two-dimensional orientation angles of the reinforcing fiber single yarns 2 to 7) in the above are calculated and the average value is calculated. When there are many reinforcing fiber single yarns crossing the selected reinforcing fiber single yarn, 20 reinforcing fiber single yarns crossing each other may be randomly selected and the average value may be measured instead of the above average value.

[0036] II. Focusing on other reinforcing fiber monofilaments, the measurement in the above-mentioned I was repeated 5 times in total, and the average value was calculated as the two-dimensional orientation angle.

[0037] The two-dimensional orientation angle indicating the fiber morphology and fiber orientation of the reinforcing fibers (Cf) in the reinforcing fiber substrate is 10 to 80°, preferably 20 to 70°, more preferably 30 to 60°, and the closer to 45°, which is an ideal angle, the more preferred. If the two-dimensional orientation angle is less than 10° or greater than 80°, it means that the reinforcing fibers are more present in bundles, which not only reduces the mechanical properties, but also damages the two-dimensional isotropy, and the reinforcing fibers in the thickness direction cannot be ignored, the density of the sheet is inconsistent, there is a deviation, etc., the texture is deteriorated, and the handling property is deteriorated when manufacturing the core material.

[0038] In order to make the core material exert high compressive strength and shear strength, when the column axis direction of the unit is set to 0°, the average fiber orientation angle of the reinforcing fiber (Cf) in the in-plane direction of the unit wall is preferably 0° to 45°, more preferably 5° to 40°. By keeping the average fiber orientation angle within this range, in addition to high mechanical properties, the linear expansion coefficient in the thickness direction of the core material is also reduced, so when molding or exposed to repeated high and low temperature environments, it is possible to suppress the generation of cracks caused by thermal shrinkage differences. Therefore, it can be particularly suitable for thick-walled skin-core structures or large structures with a core material thickness greater than 50 mm.

[0039] Specifically, there is no particular limitation on the method for measuring the average fiber orientation angle of the in-plane direction of the unit wall surface of the reinforcing fiber (Cf). For example, in addition to taking the column axis direction of the unit as the reference 0°, a method for observing the orientation of the reinforcing fiber (Cf) from the surface of a sample cut from a sheet or core material in the same manner as the above-mentioned two-dimensional orientation angle can be exemplified. In this case, it is easier to observe the reinforcing fiber (Cf) by grinding the sample surface to expose the fiber, so it is preferred. In addition, a method for observing the orientation of the reinforcing fiber (Cf) using transmitted light for a sample cut from a sheet or core material can be exemplified.

[0040] The average fiber orientation angle in the in-plane direction of the cell wall surface of the reinforcing fibers (Cf) will be described using the drawings. Figure 5 Schematic diagram showing the dispersion state of the reinforcing fibers when the cell wall cut out from the core material of the present invention is observed from a direction perpendicular to the cell wall. Focusing on the reinforcing fiber monofilament 16, the fiber orientation angle is defined as an angle θ1 of 0° or more and 90° or less, of the two angles formed between the reinforcing fiber monofilament 16 and the column axis direction 18 of the cell.

[0041] In order to make the two-dimensional orientation angle and the average fiber orientation angle θ1 in the in-plane direction of the unit wall surface close to the ideal angle, it can be achieved by dispersing the reinforcing fibers and arranging them in a plane when manufacturing the reinforcing fiber substrate. In order to improve the dispersion of the reinforcing fibers, in the dry method, examples include a method of setting open fiber strips, a method of further vibrating the open fiber strips, a method of further narrowing the holes of the card, a method of adjusting the rotation speed of the card, etc. For the wet method, examples include a method of adjusting the stirring conditions when dispersing the reinforcing fibers, a method of diluting the concentration, a method of adjusting the viscosity of the solution, a method of suppressing eddy currents when conveying the dispersion, etc. In addition, in order to arrange in a plane, for the dry method, examples include a method of using static electricity when collecting reinforcing fibers, a method of using rectified air, a method of adjusting the traction speed of the conveyor, etc. For the wet method, examples include a method of preventing the dispersed reinforcing fibers from re-agglomerating using ultrasound, a method of adjusting the filtration speed, a method of adjusting the aperture of the conveyor, a method of adjusting the traction speed of the conveyor, etc. There are no special limitations on these methods, and they can also be achieved by controlling other manufacturing conditions while confirming the state of the reinforcing fiber substrate. In particular, in the case of manufacturing by a wet method, examples such as using Figure 3 A method for manufacturing a papermaking substrate as shown. By increasing the concentration of the input fiber, the mass per unit area of ​​the obtained reinforcing fiber substrate can be increased. Furthermore, the mass per unit area can also be adjusted by adjusting the flow rate (flow rate) of the dispersion and the speed of the mesh conveyor. For example, the speed of the mesh conveyor can be kept constant, and the flow rate of the dispersion can be increased to increase the mass per unit area of ​​the obtained reinforcing fiber substrate. On the contrary, by keeping the speed of the mesh conveyor constant and reducing the flow rate of the dispersion, the mass per unit area of ​​the obtained reinforcing fiber substrate can also be reduced. In addition, by adjusting the speed of the mesh conveyor relative to the flow rate of the dispersion, the orientation of the fibers can also be controlled. For example, by increasing the speed of the mesh conveyor relative to the flow rate of the dispersion, it is easy to orient the fibers in the obtained reinforcing fiber substrate toward the pulling direction of the mesh conveyor, and the reinforcing fibers (Cf) can be configured so that the average fiber orientation angle is less than 45°.

[0042] From the viewpoint of both mechanical properties and core formability, the mass ratio of the reinforcing fiber substrate in the sheet used in the core material of the present invention is preferably 10 to 60 mass%, more preferably 12 to 50 mass%, and further preferably 15 to 40 mass% relative to 100 mass% of the sheet. In the sheet of the present invention, it is necessary to impregnate the resin in the voids of the reinforcing fiber substrate, and the impregnation rate is preferably 30 to 100 vol%, more preferably 40 to 100 vol%, and further preferably 50 to 100 vol%. If the impregnation rate is within the preferred range, it can be used without damaging the effect of the present invention, that is, the operability of the sheet and the formability of the core material. In order to make the core material exert high mechanical properties, the proportion of the unimpregnated part of the sheet (void ratio) is preferably 5% or less, and more preferably 2% or less. In addition, from the viewpoint of improving the lightness of the core material of the present invention, the volume ratio of the reinforcing fiber in the sheet when the impregnation rate is converted to 100 vol% is preferably 50 vol% or less, more preferably 40 vol% or less, and further preferably 10 to 30 vol%.

[0043] There is no particular limitation on the method for measuring the impregnation rate, and for example, the following simple method can be used for measurement. First, there can be exemplified a method of measuring the total area of ​​voids by observing the cross section of the sheet and measuring the total area of ​​voids from a microscope photograph, a method of measuring the total area of ​​voids by the ratio of the thickness h0 of the sheet at 23°C to the thickness hc0 after press molding at 23°C (hc0 / h0), and a method of measuring the total area of ​​voids by the ratio of the theoretical density calculated from the use ratio of each material to the bulk density of the sheet. Here, a method of observing the cross section in the thickness direction of the sheet, measuring the area of ​​the voids in the cross section and the area of ​​the entire cross section and calculating the total area of ​​the cross section is specifically described. That is, a sheet is embedded with a thermosetting resin such as epoxy resin, the surface in contact with the end of the cross section of the sheet is polished, and a range of about 500 to 1000 μm in width is observed with an optical microscope or an electron microscope. In terms of contrast ratio, the area of ​​the resin-impregnated portion and the area of ​​the resin-unimpregnated portion is calculated, and the resin impregnation rate is calculated by the following formula. At this time, the total area of ​​the reinforcing fiber substrate is obtained by subtracting the area of ​​the resin-impregnated portion and the area of ​​the resin-unimpregnated portion from the cross-sectional area of ​​the observed portion of the sheet.

[0044] Resin impregnation rate (%) = 100 × (total area of ​​resin impregnated parts) / (total area of ​​resin impregnated parts + area of ​​resin non-impregnated parts)

[0045] The bulk density of the sheet can be determined from the volume and mass of the sheet at 23°C. The preferred bulk density of the sheet is 0.8 to 1.6 g / cm 3 , more preferably 0.9 to 1.4 g / cm 3 , more preferably 1.0 to 1.3 g / cm 3If the bulk density is within the preferred range, the molded product using the core material of the present invention can ensure sufficient lightness. Similarly, the unit area mass of the sheet is preferably 10 to 500 g / m 2 , more preferably 30 to 400 g / m 2 , more preferably 100 to 300 g / m 2 .

[0046] In order to ensure operability in the core material molding process, the higher the tensile strength σ of the sheet material, the more it can provide a high-speed and economical molding process, but it is preferably at least 10MPa at room temperature (23°C). When it is less than 10MPa, problems such as sheet breakage sometimes occur during the operation of core material molding. In addition, the tensile strength σ of the sheet material is more preferably less than 1000MPa at room temperature (23°C). If the tensile strength σ of the sheet material is too high, the toughness is too strong, and sometimes the operability during core material molding deteriorates. The tensile strength σ of the sheet material is measured, for example, by cutting a test piece from the sheet material, and measuring the tensile properties according to ISO527-3 method (1995). When the arbitrary direction of the test piece is set to the 0° direction, test pieces cut in four directions of +45°, -45°, and 90° are made, and the number of measurements in each direction is set to n=5, and the average value can be set as the tensile strength.

[0047] In addition, from the perspective of operability in the core material molding process, the thickness h0 (mm) of the sheet at 23°C is preferably 0.02 to 1 mm. If h0 is less than 0.02 mm, the sheet may break during the conveying of the sheet or the core material molding process. When h0 is greater than 1 mm, the fiber orientation along the thickness direction becomes larger, and the sheet expands in thickness during the core material molding process, sometimes damaging the quality of the molded product due to mold deformation. Therefore, the thickness h0 of the sheet used in the present invention at 23°C is preferably 0.05 to 0.8 mm, and more preferably 0.1 to 0.6 mm.

[0048] The coverage factor of the reinforcing fibers in the sheet used in the core material of the present invention is preferably 95% or more, more preferably 99% or more. The coverage factor here refers to the value defined by the following formula when the area of ​​the area S1 is set on the sheet and the area of ​​the voids formed by the reinforcing fibers within the area S1 or the area of ​​the portion filled with only resin without reinforcing fibers is set as S2.

[0049] Coverage factor (%) = [(S1-S2) / S1] × 100

[0050] In order for the material to exhibit high compression characteristics, or to exhibit high resistance to compression collapse when formed with a skin or used as a structural component, the cell wall needs to have a high elastic modulus. Therefore, the core material preferably has an elastic modulus of 1 GPa or more at room temperature (20°C ± 15°C), and more preferably has an elastic modulus of 1 GPa or more at 120 to 200°C, which is a general molding temperature of the skin-core structure. Here, the elastic modulus refers to the storage modulus measured by dynamic mechanical analysis (DMA), which is the storage modulus at room temperature or the molding temperature (120 to 200°C) of the skin-core structure obtained by collecting the cell wall from the core material, taking the thickness direction of the core material (the column axis direction of the cell) as the length direction of the test piece, using DMA Q800 (manufactured by TA Instruments), setting the heating rate to 5°C / min, the frequency to 1 Hz, and performing DMA measurement in single cantilever mode.

[0051] The matrix resin of the sheet used in the core material of the present invention can be a thermoplastic resin or a thermosetting resin. As the thermoplastic resin, for example, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyoxymethylene, polyamide 6, polyamide 66, polyamides such as polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, polyarylether sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyaryletherketone, polyarylate, polyethernitrile, phenoxy resin, etc. can be listed. In addition, these thermoplastic resins can also be copolymers or modified bodies and / or resins mixed with two or more of these. Among them, at least one thermoplastic resin selected from the group consisting of polyarylether sulfide, polyetherimide, polyethersulfone, polysulfone, and polyaryletherketone is more preferred in view of heat resistance and mechanical properties.

[0052] The thermosetting resin may be, for example, an unsaturated polyester resin, a vinyl ester resin, an epoxy resin, a phenolic resin, a urea resin, a melamine resin, a thermosetting polyimide resin, a BT resin, a cyanate ester resin, a bismaleimide resin, a benzoxazine resin, or a copolymer thereof, a modified product thereof, and / or a resin obtained by mixing two or more of these. Among them, from the perspective of heat resistance and mechanical properties, at least one thermosetting resin selected from epoxy resin, phenolic resin, benzoxazine resin, BT resin, cyanate ester resin, bismaleimide resin, and polyimide resin is more preferred.

[0053] The resin component used in the present invention may be a mixture of a thermoplastic resin matrix mixed with a thermosetting resin, or a mixture of a thermoplastic resin matrix mixed with a thermosetting resin. In particular, when a thermosetting resin is used, it is preferred to use thermoplastic resin particles as interlayer particles from the viewpoint of improving impact strength. Furthermore, the resin component may further contain fillers such as mica, talc, kaolin, hydrotalcite, sericite, bentonite, burnt vermiculite, sepiolite, smectite, montmorillonite, wollastonite, silica, calcium carbonate, glass beads, glass flakes, glass microspheres, clay, molybdenum disulfide, titanium oxide, zinc oxide, antimony oxide, calcium polyphosphate, graphite, barium sulfate, magnesium sulfate, zinc borate, calcium borate, aluminum borate whisker, potassium titanate whisker, and polymer compounds, as well as conductive materials such as metals, metal oxides, carbon black, and graphite powder, halogen flame retardants such as brominated resins, antimony flame retardants such as antimony trioxide or antimony pentoxide, phosphorus flame retardants such as ammonium polyphosphate, aromatic phosphates, and red phosphorus, organic acid metal salt flame retardants such as borate metal salts, carboxylic acid metal salts, and aromatic sulfonyl imide metal salts, zinc borate, zinc oxide, and graphite powder. Inorganic flame retardants such as zinc and zirconium compounds, nitrogen flame retardants such as cyanuric acid, isocyanuric acid, melamine, melamine cyanurate, melamine phosphate and guanidine nitride, polyfluorine flame retardants such as PTFE, siloxane flame retardants such as polyorganosiloxane, and metal hydroxide flame retardants such as aluminum hydroxide and magnesium hydroxide, as well as other flame retardants, flame retardant additives such as cadmium oxide, zinc oxide, cuprous oxide, cupric oxide, ferrous oxide, ferric oxide, cobalt oxide, manganese oxide, molybdenum oxide, tin oxide and titanium oxide, pigments, dyes, lubricants, release agents, compatibilizers, dispersants, crystal nucleating agents such as mica, talc and kaolin, plasticizers such as phosphate esters, heat stabilizers, antioxidants, anti-coloring agents, ultraviolet absorbers, flow modifiers, foaming agents, antibacterial agents, vibration damping agents, deodorants, sliding modifiers, and antistatic agents such as polyether ester amides, etc. In particular, when the application is electric and electronic equipment, automobiles, airplanes, etc., flame retardancy may be required, and it is preferable to add a phosphorus-based flame retardant, a nitrogen-based flame retardant, or an inorganic flame retardant.

[0054] <Skin-core structure>

[0055] The core material of the present invention is not particularly limited, but is usually used as a skin-core structure with a skin material bonded to at least one side, preferably both sides, of the end face (core opening face) of the columnar unit opening. There is no particular limitation on the method of joining the skin material and the core material, and examples include joining with an adhesive and heat fusion. For example, an adhesive sheet and a skin material can be arranged on both sides of the core material, and they can be bonded to the core material while being heated and cured. In addition, there is no particular limitation on the joining process, and molding can be performed by vacuum bag molding, autoclave molding, press molding, etc.

[0056] The fiber-reinforced composite material for leather material is preferably formed by a prepreg in which a resin (Sr) is impregnated in the reinforcing fiber (Sf). The morphology of the reinforcing fiber is not limited to its shape and arrangement. For example, a single direction, a random direction, a sheet, a felt, a fabric, and a combined tape (group-shaped) can also be used. Among them, a two-dimensional fabric can be preferably used, and there is no particular limitation on the fabric structure. Fabrics such as plain weave, twill weave, gauze weave, and satin weave are preferred. In particular, the plain weave structure is suitable in that it is easy to manufacture a thin molded body. The yarn of the fabric is composed of a fiber bundle, but the number of filaments in a fiber bundle is preferably in the range of 2500 to 50000. If it is less than 2500, the fiber arrangement is easy to be tortuous, which is easy to become the cause of reduced strength. In addition, if it is greater than 50000, it is difficult to impregnate the resin when making the prepreg or molding. More preferably, the range of 2800 to 25000. In particular, from the viewpoint of improving the surface smoothness of the honeycomb skin surface, the number of filaments is preferably 5,000 or more.

[0057] The prepreg preferably has a weight per unit area of ​​150 to 550 g / m 2 Thus, a leather material with excellent mechanical strength can be obtained. If the unit area mass of the reinforcing fiber is less than 150g / m 2 If the mechanical strength is greater than 550g / m 2 The weight per unit area of ​​the reinforcing fiber is more preferably 170 to 500 g / m 2 If the mass fraction of the reinforcing fibers in the prepreg is less than 40 mass %, the rigidity of the obtained skin material may be insufficient, and if it is greater than 85 mass %, voids may be easily generated in the obtained skin material.

[0058] As a specific example of the reinforcing fiber of the above-mentioned prepreg, carbon fiber, graphite fiber, aramid fiber, silicon carbide fiber, aluminum oxide fiber, boron fiber, tungsten carbide fiber, glass fiber, etc. can be listed. Reinforcing fiber can also be used in combination. Among them, carbon fiber or graphite fiber that has good specific strength and specific elastic modulus and is considered to have a greater contribution to lightweight is preferred for the present invention. Carbon fiber and graphite fiber can use all kinds of carbon fiber and graphite fiber according to the purpose, but from the original tensile strength of the fiber and the high impact resistance when becoming a skin-core structure, it is preferred to use the strand strength in the strand tensile test to be 3000MPa or more and 7500MPa or less and the elastic modulus to be 200GPa or more and 600GPa or less. In addition, the so-called strand tensile test refers to the test based on JIS R7601 (2006) in which the matrix resin of the following composition is impregnated in the bundled carbon fiber, and after curing for 35 minutes at a temperature of 130°C.

[0059] The number of carbon fiber filaments is preferably 1000 to 100000, more preferably 3000 to 50000. If the number of carbon fiber filaments is less than 1000, the prepreg operation becomes complicated, and if it is more than 100000, it is difficult to impregnate the filaments with resin, and impregnation failure may occur.

[0060] The skin-core structure of the present invention preferably has an average peel torque M (climbing drum peel test strength) of 30 N·m / m or more between the skin and the core as measured by ASTM D1781 (2004), and more preferably 35 N·m / m or more. By having a roller peel strength of 30 N·m / m or more, the skin-core structure can withstand high loads, and because of the lightweight effect, it is suitable as a structural component for flying objects such as aircraft. The higher the roller peel strength, the stronger the adhesion between the skin and the core, so no upper limit is set.

[0061] The reinforcing fiber (Sf) of the skin material composed of the above-mentioned fiber-reinforced composite material preferably has a tensile elastic modulus E of 200 GPa or more and a breaking strain strength W of 40 MPa or more. By using reinforcing fibers with a high tensile elastic modulus, high strength can be obtained in a roller peel test, which is one of the evaluations of the adhesion between the skin material and the core material. In addition, the breaking strain strength mentioned here refers to the value calculated using the tensile strength (σ: MPa) and elastic modulus (E: MPa) measured according to JIS-R7601 (2006) according to the following formula: W = σ2 / 2E. As specific examples of such high-strength and high-elongation carbon fibers, for example, commercially available products of carbon fibers include "TORECA (registered trademark)" T800G-24K, "TORECA (registered trademark)" T800S-24K, "TORECA (registered trademark)" T700G-24K, "TORECA (registered trademark)" T700S-24K, "TORECA (registered trademark)" T300-3K, and "TORECA (registered trademark)" T1100G-24K (all manufactured by Toray Industries, Inc.).

[0062] The coverage factor of the prepreg used for the above-mentioned skin material is preferably 95% or more. When the coverage factor is insufficient, pits are sometimes generated on the surface of the skin material of the molded body, voids are generated inside, and the roller peel strength becomes smaller. Here, the so-called coverage factor, like the above-mentioned sheet, refers to the proportion of the area where the reinforcing fibers exist in the total area of ​​the prepreg. In particular, in the case of a prepreg using a woven reinforcing fiber substrate, due to the presence of weave holes (gaps formed between woven yarns), the coverage factor generally tends to be lower than that of a prepreg using a reinforcing fiber substrate in which the reinforcing fibers are arranged in one direction. By using a woven prepreg with a coverage factor of 95% or more as the surface surface, a skin-core structure with excellent strength is obtained because the skin material has fewer defects.

[0063] Regarding the flammability of the skin-core structure of the present invention, the burning time can be measured according to FAR25.853 Appendix F. In addition, regarding the quality of its burning time, according to Advisory Circular (AC) 25.853-1a(1)i "Flammability Requirements for Aircraft Seat Cushions" issued by the Federal Aviation Administration, the burning time of the skin-core structure after the ignition source is extinguished is 30 seconds or less, preferably 15 seconds or less. When the burning time of the skin-core structure is longer than 30 seconds, the flammability is poor, that is, it is burned, which is undesirable from a safety point of view. Regarding the length of the burning time of the skin-core structure, no restriction is set because the shorter the burning time, the better the flammability. In the FAR25.853 Appendix F of the above-mentioned Federal Aviation Regulations (FAR), the test piece is fixed in a vertical state with its long side, and a burner is used to burn the test piece from directly below with a flame directed toward the center of the bottom side of the test piece to measure and evaluate the test piece. In this evaluation method, the distance between the test piece and the burner is set to 19 mm, and the time for the flame to be emitted from the test piece during the 60-second baking of the test piece is measured as the burning time.

[0064] The resin (Sr) used for the prepreg of the leather material can be a thermoplastic resin or a thermosetting resin. As the thermoplastic resin, for example, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyoxymethylene, polyamide 6, polyamide 66, polyamides such as polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, polyarylether sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyaryletherketone, polyarylate, polyethernitrile, phenoxy resin, etc. can be listed. In addition, these thermoplastic resins can also be copolymers or modified bodies and / or resins mixed with two or more of these. Among them, at least one thermoplastic resin selected from the group consisting of polyarylether sulfide resin, polyetherimide resin, polyethersulfone resin, polysulfone resin, and polyaryletherketone resin is more preferred in view of heat resistance and mechanical properties.

[0065] The thermosetting resin may be, for example, an unsaturated polyester resin, a vinyl ester resin, an epoxy resin, a phenolic resin, a urea resin, a melamine resin, a thermosetting polyimide resin, a BT resin, a cyanate resin, a bismaleimide resin, a benzoxazine resin, or a copolymer or a modified product thereof and / or a resin obtained by mixing two or more of these. Among them, from the perspective of heat resistance and mechanical properties, at least one thermosetting resin selected from epoxy resin, phenolic resin, cyanate resin, bismaleimide resin, and polyimide resin is more preferred.

[0066] Furthermore, other fillers or additives may be appropriately contained within the scope of not impairing the purpose of the present invention, depending on the application, etc. For example, as the resin of the above-mentioned prepreg, a mixture of a thermoplastic resin mixed with a thermosetting resin, or a mixture of a thermoplastic resin mixed with the above-mentioned thermosetting resin may be used. In particular, when the application is electrical and electronic equipment, automobiles, aircraft, etc., flame retardancy is sometimes required, so it is preferable to add a phosphorus flame retardant, a nitrogen flame retardant, or an inorganic flame retardant.

[0067] The skin-core structure of the present invention preferably has a heat-resistant temperature Ts of the resin constituting the skin material and a heat-resistant temperature Tc of the resin constituting the sheet material of the core material of Ts≤Tc. The heat-resistant temperature mentioned here refers to the melting point in the case of a crystalline resin, and refers to the glass transition temperature in the case of an amorphous resin or a thermosetting resin. By Ts≤Tc, it becomes easy to maintain the shape of the core material, and it is easy to obtain a molded body of good quality, or it can be molded in a short time. In addition, it is also easy to heat-weld the skin material and the core material, thereby simplifying the molding process, so it is preferred. Tc is preferably higher than Ts by more than 10°C, and more preferably Tc is higher than Ts by more than 20°C.

[0068] In order to exert high bonding strength, the skin-core structure of the present invention preferably has an interface layer formed by mixing the resin (Cr) of the core material and the resin (Sr) of the skin material. The mixing mentioned here refers to the state in which the resin (Cr) and the resin (Sr) are uniformly dispersed with each other, which includes not only the state in which the resin (Cr) and the resin (Sr) are mixed when they are compatible with each other, but also the dispersed state in which the resin (Cr) and the resin (Sr) are mixed with each other even if they are incompatible with each other. There is no particular limitation on the method for measuring the mixed interface layer. For example, it can be determined by analyzing the cross-section of the skin-core structure using known methods such as chemical composition mapping methods such as microscopic IR, SEM-EDX, TEM-EDX, TEM-EELS, or viscoelastic mapping methods such as VE-AFM.

[0069] In the skin-core structure of the present invention, it is preferred that a portion of the discontinuous fibers (Cf) contained in the cell walls of the core material enter the skin material. The state in which the fibers (Cf) enter the skin material is exemplified in Figure 6In the manner shown. That is, across the interface layer formed by the resin (Sr) 22 of the skin material and the resin (Cr) 20 of the core material, there exists a fiber (Cf) 19 in contact with both the resin (Sr) 22 and the resin (Cr) 20. The maximum penetration distance of the fiber (Cf) 19 into the skin material is preferably greater than 5 μm, and more preferably greater than 10 μm. Regarding the penetration distance of the fiber (Cf) 19 into the skin material, it is defined as the shortest distance from an imaginary plane (a horizontal plane parallel to the skin material) at the depth of the front end of a certain fiber (Cf) 19 that penetrates the skin material, which exists on the side of the resin (Sr) 22 of the skin material (Cf) 19 invading the skin material, to the boundary between the resin (Sr) 22 of the skin material and the resin (Cr) 20 of the core material, Figure 6 In the case of the fiber (Cf) 19a in the skin material, the distance is represented by symbol 23. And the maximum value among the measured invasion distances is taken as the maximum invasion distance. The maximum invasion distance of the fiber (Cf) into the skin material can be specifically measured as follows. Cut out the joining part of the skin material and the core material of the structure, and use a laser microscope to photograph any 10 places (10 images) at a magnification of 1000 times for its thickness direction section. Based on the obtained images, the invasion distance of each single fiber of the fiber (Cf) entering the skin material is calculated, and the maximum value is taken as the maximum invasion distance.

[0070] When the resin (Sr) of the skin material is a thermosetting resin, it is preferred to place the uncured prepreg on the end surface of the core material, and heat and pressurize while bonding to perform so-called co-cure. Compared with the so-called co-bond method of pre-curing the skin material and bonding it to the core material using an adhesive, the molding times are small, so it is advantageous in terms of molding cost and can be molded in a short time. Furthermore, by co-curing the skin material, the fiber (Cf) can enter the skin material, so a strong bond can be formed.

[0071] When the resin (Sr) of the skin material is a thermoplastic resin, it is preferably bonded to the core material while being heated and pressurized at a temperature above the melting point of the resin (Sr). By co-curing the skin material, the fiber (Cf) easily enters the resin (Sr) of the skin material, and a strong bond between the skin material and the core material can be formed.

[0072] Example

[0073] The materials used in Examples and Comparative Examples are as follows.

[0074] [Reinforcement fiber 1]

[0075] A copolymer containing polyacrylonitrile as a main component was spun, calcined and surface-oxidized to obtain a continuous carbon fiber having a total of 12,000 filaments. The properties of the continuous carbon fiber are shown below.

[0076] Single fiber diameter: 7μm

[0077] Specific gravity: 1.8

[0078] Tensile strength: 4600MPa

[0079] Tensile elastic modulus: 220GPa

[0080] 〔PEKK resin〕

[0081] A sheet with a mass of 60 g / m2 was prepared from a polyetherketoneketone resin (KEPSTAN (registered trademark) 7002 manufactured by Alkama Co., Ltd.). 2 of resin film.

[0082] 〔PPS resin〕

[0083] A polyphenylene sulfide resin (Toray Industries, Inc. "Toray Na" (registered trademark) M2888) with a mass per unit area of ​​60 g / m 2 of resin film.

[0084] 〔PEI resin〕

[0085] A polyetherimide resin (ULTEM (registered trademark) 1000 manufactured by SABIC) with a mass per unit area of ​​60 g / m 2 of resin film.

[0086] [Reinforcement fiber base material 1]

[0087] The carbon fiber 1 was cut into 6 mm pieces using a box cutter to obtain chopped carbon fibers. A dispersion having a concentration of 0.1% by mass was prepared from water and a surfactant (polyoxyethylene lauryl ether (trade name) manufactured by Nacalaitex Co., Ltd.). The dispersion and the chopped carbon fibers were used to prepare the chopped carbon fibers. Figure 3 The reinforcing fiber base material is manufactured using the manufacturing apparatus for the reinforcing fiber base material shown. Figure 3 The manufacturing device shown comprises: a cylindrical container with a diameter of 1000 mm having an open cock at the bottom of the container as a dispersion tank, and a linear conveying section (inclination angle 30°) connecting the dispersion tank and the papermaking tank. A stirrer is attached to the opening on the top of the dispersion tank, and chopped carbon fibers and a dispersion liquid (dispersion medium) can be added from the opening. The papermaking tank is a tank having a mesh conveyor (mesh conveyor) with a papermaking surface with a width of 500 mm at the bottom, and the mesh conveyor is connected to a conveyor capable of transporting a carbon fiber substrate (papermaking substrate). Papermaking is carried out with a carbon fiber concentration of 0.05% by mass in the dispersion. The carbon fiber substrate after papermaking is dried in a drying furnace at 200°C for 30 minutes to obtain a reinforcing fiber substrate 1. The obtained unit area mass is 40g / m 2 .

[0088] [Reinforcement fiber base material 2]

[0089] A reinforcing fiber substrate 2 was prepared in the same manner as the reinforcing fiber substrate 1 described above, except that the speed of the mesh conveyor during papermaking was adjusted to 4 times the flow rate of the dispersion.

[0090] [Sheet 1]

[0091] A reinforcing fiber substrate 1 as a reinforcing fiber substrate and a PEKK resin as a resin film are arranged in the order of [resin film / reinforcing fiber substrate / resin film] to produce a laminate. Then, a sheet 1 is obtained through the following steps (I) to (IV).

[0092] (I) The laminate was placed in a press-molding cavity preheated to 250° C., and the mold was closed and maintained for 120 seconds.

[0093] (II) A pressure of 5 MPa was then applied, and the temperature was raised to 350° C. and maintained for 10 minutes.

[0094] (III) The cavity temperature was cooled to 50°C while maintaining the pressure.

[0095] (IV) Open the mold and take out the sheet.

[0096] [Sheet 2]

[0097] A reinforcing fiber substrate 1 as a reinforcing fiber substrate and a PPS resin as a resin film are arranged in the order of [resin film / reinforcing fiber substrate / resin film] to produce a laminate. Then, a sheet 2 is obtained through the following steps (I) to (V).

[0098] (I) The laminate was placed in a press-molding cavity preheated to 200° C., and the mold was closed and maintained for 120 seconds.

[0099] (II) A pressure of 5 MPa was then applied, and the temperature was raised to 300° C. and maintained for 10 minutes.

[0100] (III) The cavity temperature was cooled to 50°C while maintaining the pressure.

[0101] (IV) Open the mold and take out the sheet.

[0102] [Sheet 3]

[0103] A reinforcing fiber substrate 2 as a reinforcing fiber substrate and a PEKK resin as a resin film are arranged in the order of [resin film / reinforcing fiber substrate / resin film] to produce a laminate. Then, a sheet 1 is obtained through the following steps (I) to (IV).

[0104] (I) The laminate was placed in a press-molding cavity preheated to 250° C., and the mold was closed and maintained for 120 seconds.

[0105] (II) A pressure of 5 MPa was then applied, and the temperature was raised to 350° C. and maintained for 10 minutes.

[0106] (III) The cavity temperature was cooled to 50°C while maintaining the pressure.

[0107] (IV) Open the mold and take out the sheet.

[0108] [Sheet 4]

[0109] The reinforcing fiber 1 was cut into 25 mm long pieces, and the chopped carbon fiber bundles were dispersed in a manner that the carbon fiber bundles were distributed in random directions to prepare 40 g / m 2 A reinforcing fiber substrate is prepared, and a PEKK resin as a resin film is arranged in the order of [resin film / reinforcing fiber substrate / resin film] to produce a laminate. Then, the sheet 4 is obtained through the following steps (I) to (IV).

[0110] (I) The laminate was placed in a press-molding cavity preheated to 250° C., and the mold was closed and maintained for 120 seconds.

[0111] (II) A pressure of 5 MPa was then applied, and the temperature was raised to 350° C. and maintained for 10 minutes.

[0112] (III) The cavity temperature was cooled to 50°C while maintaining the pressure.

[0113] (IV) Open the mold and take out the sheet.

[0114] [Sheet 5]

[0115] A reinforcing fiber substrate 1 as a reinforcing fiber substrate and a PEI resin as a resin film are arranged in the order of [resin film / reinforcing fiber substrate / resin film] to produce a laminate. Then, a sheet 5 is obtained through the following steps (I) to (V).

[0116] (I) The laminate was placed in a press-molding cavity preheated to 250° C., and the mold was closed and maintained for 120 seconds.

[0117] (II) A pressure of 5 MPa was then applied, and the temperature was raised to 350° C. and maintained for 10 minutes.

[0118] (III) The cavity temperature was cooled to 50°C while maintaining the pressure.

[0119] (IV) Open the mold and take out the sheet.

[0120] [Honeycomb core 1]

[0121] The honeycomb core is made by the corrugation method using the sheet 1 as the base material. First, the corrugated plate is bent while the base material is heated, and multiple corrugated plates are stacked into blocks with each valley and top portion staggered by half the wave pitch with adhesive sandwiched therebetween, and then heated and pressed to bond, thereby making a honeycomb core 1 (thickness 12.7 mm, mass per unit volume 45 kg / m 3 ).

[0122] [Honeycomb core 2]

[0123] The honeycomb core 2 (thickness 12.7 mm, mass per unit volume 50 kg / m2) was prepared by the same process as the honeycomb core 1 except that the sheet 2 was used as the base material. 3 ).

[0124] [Honeycomb core 3]

[0125] The honeycomb core 3 (thickness 12.7 mm, mass per unit volume 45 kg / m) was prepared by the same process as the honeycomb core 1 except that the sheet 3 was used as the base material. 3 ).

[0126] [Honeycomb core 4]

[0127] The honeycomb core is manufactured by the same process as the honeycomb core 1 except that the sheet 4 is used as the base material. However, when the base material is bent into a corrugated plate, holes are formed in the sheet or uneven deformation is formed to form a resin-only area, and the honeycomb core cannot be manufactured even if the processing conditions are adjusted.

[0128] [Honeycomb core 5]

[0129] Aramid honeycomb (manufactured by Showa Aircraft Industry Co., Ltd., model: SAH1 / 8-3.0, thickness 12.7 mm, mass per unit volume 48 kg / m 3 ) as the honeycomb core 5.

[0130] [Honeycomb core 6]

[0131] A honeycomb core 6 (thickness 12.7 mm, mass per unit volume 50 kg / m2) was produced by the same process as the honeycomb core 1 except that the sheet 5 was used as the base material. 3 ).

[0132] [Leather]

[0133] Use a kneader to knead the epoxy resin "Alaraplast" (Note "Registered Trademark)" MY721: 40 parts by mass, "Ebotron (Registered Trademark) manufactured by Seton Co., Ltd. ” 828: 35 parts by mass, “E-Toto (registered trademark)” 1001: 25 parts by mass, “E-toto (registered trademark)” 154: 25 parts by mass) and polyethersulfone (“E-Toto (registered trademark)” PES manufactured by Sumitomo Chemical Co., Ltd. 5003P: 5 parts by mass) was heated and kneaded to uniformly dissolve polyethersulfone, and then polyamide particles (Toray Industries, Inc. "Amiran (registered trademark)" SP-500: 13 parts by mass) and a curing agent (Seika Co., Ltd. "Seika Curia (registered trademark)" S: 36 parts by mass) were kneaded in a kneader to prepare an uncured epoxy resin composition, from which an epoxy resin film was prepared using a knife coater. Next, the epoxy resin film was overlapped on both sides of the reinforcing fiber fabric and coated with a hot The prepreg 1 having a fiber volume content of 60% was prepared by impregnating the prepreg with the resin composition while heating and pressurizing the prepreg with the roll. In addition, as the reinforcing fiber fabric, a plain weave fabric CF6273H (fiber mass per unit area 193 g / m2) made of carbon fiber "Toreka (registered trademark)" T700G-12K (number of fibers 12,000, tensile strength 4.9 GPa, tensile elastic modulus 240 GPa, tensile elongation 2.1%) manufactured by Toray Industries, Ltd. was used. 2 ).

[0134] The produced prepreg 1 was stacked in a two-layer symmetrical structure of (±45°) / (0° / 90°), and heated under pressure at 0.30 MPa and 180° C. for 2 hours in an autoclave to obtain a skin material.

[0135] The evaluation methods of the structures, physical properties, etc. in each of the Examples and Comparative Examples are as follows.

[0136] [Evaluation of the length of reinforcing fibers contained in the sheet]

[0137] The sheet was heated and pressed at 350°C to produce a film with a thickness of 50 μm. 400 reinforcing fibers in the film were randomly selected and their lengths were measured to 1 μm units using an optical microscope to measure the fiber length and its ratio. Furthermore, the number of reinforcing fibers was counted at 0.25 mm intervals such as less than 0.25 mm, 0.25 mm or more and less than 0.5 mm, and 0.5 mm or more and less than 0.75 mm to evaluate the fiber length distribution.

[0138] [Measurement of two-dimensional orientation angle of reinforcing fibers in sheets]

[0139] like Figure 2As shown, the sheet is sandwiched between two stainless steel meshes (plain weave shape with 50 holes per 2.5 cm), and the screws are adjusted to fix it so that the sheet cannot move. It is heated at 500°C in air for 1 hour to burn off the resin component. Remove the stainless steel mesh, observe the obtained reinforcing fiber substrate under a microscope, randomly select one reinforcing fiber monofilament, and measure the two-dimensional orientation angle formed by it and another reinforcing fiber monofilament that crosses the reinforcing fiber monofilament by image observation. The orientation angle adopts the angle (acute angle side) of 0° or more and 90° or less of the two angles formed by the two reinforcing fiber monofilaments that cross. The number of measurements of the two-dimensional orientation angle of each selected reinforcing fiber monofilament is n=20. A total of 5 reinforcing fiber monofilaments are selected for the same measurement, and their average value is used as the two-dimensional orientation angle.

[0140] [Sheet coverage factor (%)]

[0141] The prepared sheet was used to capture an image using an X-ray CT device that was pre-set to be able to distinguish between "reinforcement fibers", "voids", and "portions filled only with resin", and the area S1 was set based on the captured image. The area of ​​the voids formed by the reinforcement fibers or the area of ​​the portion filled only with resin without the reinforcement fibers within the area S1 was taken as S2, and the calculation was performed using the following formula. The measurement was performed at any 10 locations in the sheet, and the arithmetic average thereof was taken as the cover factor.

[0142] Coverage factor = {(S1-S2) / S1}×100

[0143] [Skin-core structure]

[0144] The skin-core structure was prepared according to the following steps (1) and (2).

[0145] (1) Sample stacking

[0146] like Figure 4 As shown, an adhesive film 14 (AF555 manufactured by 3M Co., Ltd.) and a skin material 12 (with the outermost layer being ±45° relative to the honeycomb core) are respectively laminated above and below the open end of the honeycomb core 13. Figure 4 In order to clarify the structure of the skin-core structure, the honeycomb core 13, the adhesive film 14, and the skin material 12 are shown in a separated state.

[0147] (2) Sample molding

[0148] Follow the steps (a) to (d) below.

[0149] (a) An unformed body in which an adhesive film 14 and a skin material 12 are laminated on a honeycomb core 13 is placed on an aluminum tool plate coated with a release agent.

[0150] (b) After covering the unmolded body with a nylon film, the unmolded body is directly placed in an autoclave while keeping the inside of the nylon film (hereinafter referred to as the inside of the system) in a vacuum state.

[0151] (c) The pressure in the autoclave was increased to 0.15 MPa, and then the pressure in the system was returned to normal pressure. The pressure in the autoclave was then increased to 0.30 MPa, and then the temperature was started to rise.

[0152] (d) The pressure in the autoclave is maintained at 0.30 MPa until the molding is completed, and the temperature is raised to 180°C at a rate of 1.5°C / min, and then placed at 180°C for 2 hours. After the resin is cured and bonded to the honeycomb core, the temperature is lowered to room temperature at a rate of 2°C / min to form a skin-core structure.

[0153] [Compression strength]

[0154] Samples were cut out from the above-mentioned skin-core structure and tested according to MIL-STD-401 to determine the compressive strength (tested by Stabilized Compression).

[0155] Hereinafter, the honeycomb core and the skin-core structure produced in the examples and comparative examples will be described.

[0156] [Example 1]

[0157] The skin-core structure composed of the honeycomb core 1 and the skin material was manufactured by the above method. The evaluation results are shown in Table 1.

[0158] [Example 2]

[0159] The skin-core structure composed of the honeycomb core 2 and the skin material was manufactured by the above method. The evaluation results are shown in Table 1.

[0160] [Example 3]

[0161] The skin-core structure composed of the honeycomb core 3 and the skin material was manufactured by the above method. The evaluation results are shown in Table 1.

[0162] [Example 4]

[0163] The skin-core structure composed of the honeycomb core 6 and the skin material was manufactured by the above method. The evaluation results are shown in Table 1.

[0164] [Comparative Example 1]

[0165] The honeycomb core 4 was manufactured by the above method. The results are shown in Table 1.

[0166] [Comparative Example 2]

[0167] The skin-core structure composed of the honeycomb core 5 and the skin material was manufactured by the above method. The evaluation results are shown in Table 1.

[0168] By comparing Examples 1 to 4 with Comparative Example 1, it is confirmed that the reinforcing fibers in the sheet of the base material of the honeycomb core of the present invention have high dispersion based on single filaments rather than bundles, thereby improving the texture, etc., and can be smoothly manufactured even though it is an FRP honeycomb. In addition, from the comparison of Examples 1 to 4 with Comparative Example 2, it can be seen that the honeycomb core of the present invention has high mechanical properties while being lightweight.

[0169] [Table 1]

[0170]

[0171] Industrial Availability

[0172] The core material of the present invention can be well used as structural components such as automotive interior and exterior materials, solar cell reinforcements, structural materials for sports equipment, aircraft interior materials, flying object structural materials, artificial satellite frames, transportation boxes, or as structural components of aircraft propellers, aircraft floor panels, rocket fairings and rocket stage inter-parts.

[0173] Description of the accompanying drawings

[0174] 1. Reinforced fiber monofilament

[0175] 2. Reinforced fiber monofilament

[0176] 3. Reinforced fiber monofilament

[0177] 4. Reinforced fiber monofilament

[0178] 5. Reinforced fiber monofilament

[0179] 6. Reinforced fiber monofilament

[0180] 7. Reinforced fiber monofilament

[0181] 9. Stainless steel mesh

[0182] 10. Sheet

[0183] 11. Reinforced fiber substrate

[0184] 12. Leather

[0185] 13. Core material

[0186] 14. Adhesive (film)

[0187] 15. Cut out cell wall (surface perpendicular to the thickness direction)

[0188] 16. Reinforced fiber monofilament

[0189] 18. Column axis direction of the element (0 degrees)

[0190] 19. Reinforcement fiber (Cf)

[0191] 20. Resin (Cr)

[0192] 21. Reinforcement fiber (Cf)

[0193] 22. Resin (Sr)

[0194] 23. Penetration distance of reinforcing fiber (Cf) to the leather

[0195] θ. Two-dimensional orientation angle

[0196] θ1. Average fiber orientation angle in the in-plane direction of the cell wall of the reinforcing fiber (Cf)

Claims

1. A core material having a structure consisting of an aggregate of hollow columnar units partitioned by cell walls, wherein the cell walls are composed of a sheet in which discontinuous reinforcing fibers Cf are dispersed in the form of single fibers.

2. The core material according to claim 1, wherein the sheet is formed of a reinforcing fiber base material impregnated with resin Cr, the content of discontinuous reinforcing fibers Cf in the sheet is 10 to 60% by mass, and the void ratio of the portion not impregnated with resin Cr is 5% or less.

3. The core material according to claim 1, wherein when the columnar axis direction of the cell is set to 0°, the average fiber orientation angle of the reinforcing fibers Cf in the in-plane direction of the cell wall surface is 0° or more and 45° or less. 4 . The core material according to claim 1 , wherein an average value of two-dimensional orientation angles of the reinforcing fibers Cf in the sheet is 10 to 80°, and an elastic modulus of the cell wall is 1 GPa or more.

5. The core material according to any one of claims 1 to 3, wherein the reinforcing fibers Cf in the sheet are composed of 0 to 50% by mass of reinforcing fibers having a fiber length greater than 10 mm, 50 to 100% by mass of reinforcing fibers having a fiber length of 2 to 10 mm, and 1 to 50% by mass of reinforcing fibers having a fiber length less than 2 mm. 6 . The core material according to claim 1 , wherein the fiber length distribution of the reinforcing fibers Cf has at least two peaks.

7. The core material according to claim 6, wherein the fiber length distribution of the reinforcing fibers Cf has at least two peaks, one peak being in the range of 5 to 10 mm in fiber length, and the other peak being in the range of 2 to 5 mm. 8 . The core material according to claim 1 , wherein the cover factor of the reinforcing fibers Cf in the sheet is 95% or more. 9 . The core material according to claim 1 , wherein the sheet has a thickness h0 (mm) of 0.02 to 1 mm at 23° C. and a tensile strength σ of 10 MPa or more.

10. The core material according to any one of claims 1 to 3, wherein the bulk density of the sheet is 0.8 to 1.6 g / cm 3 .

11. The core material according to any one of claims 1 to 3, wherein the reinforcing fibers Cf are carbon fibers. 12 . The core material according to claim 1 , wherein the shape of the hollow columnar unit is composed of a plurality of polygonal shapes.

13. The core material according to any one of claims 1 to 3, wherein the resin Cr contains at least one resin selected from polyarylene sulfide resin, polyetherimide resin, polyethersulfone resin, polysulfone resin, polyaryletherketone resin, and polyimide resin, and the cell walls of the core material are welded and joined by the resin Cr.

14. A skin-core structure, wherein a skin material made of a fiber-reinforced composite material is joined to a core opening surface of the core material according to any one of claims 1 to 3.

15. The skin-core structure as described in claim 14, wherein the burning time after the ignition source is extinguished measured in accordance with Advisory Circular (AC) 25.853-1a(1)i is less than 30 seconds, and the resin of the skin material contains at least one resin selected from polyarylether sulfide resin, polyetherimide resin, polyethersulfone resin, polysulfone resin, polyaryletherketone resin, polyimide resin, epoxy resin, phenolic resin, cyanate ester resin and bismaleimide resin. 16 . The skin-core structure according to claim 14 , wherein the heat resistance temperature Ts of the resin Sr constituting the skin material and the heat resistance temperature Tc of the resin Cr constituting the sheet material of the core material satisfy: Ts≤Tc.

17. The skin-core structure according to claim 14 or 15, wherein the skin-core structure has an interface layer formed by mixing resin Cr and resin Sr.

18. The skin-core structure according to claim 14 or 15, having a structure in which a part of the discontinuous reinforcing fibers Cf contained in the core material enters the skin material.

19. An aircraft propeller, an aircraft floor panel, a rocket fairing or a rocket interstage, comprising the core material according to any one of claims 1 to 3 as a structural component.

Citation Information

Patent Citations

  • Honeycomb object of high-shear modulus alamide

    JP1992226745A

  • Molded product having hollow structure and process for producing same

    CN104781065A

  • Sandwich structure and integrally formed article using same, and methods for production thereof

    CN111452445A

  • Prepreg

    JP2013166923A

  • Core member made of a composite plastic material, and method for the production thereof

    US20190329512A1